Preparation and application of a flexible biosensor with high mechanical strength

Through the combination technology of chitosan and calcium carbonate film, a high mechanical strength flexible biosensor is formed, which solves the problems of low mechanical strength and poor stability of traditional sensors, realizes sweat detection and sweat volume statistics, and reduces manufacturing costs.

CN115791772BActive Publication Date: 2024-11-05BEIJING INFORMATION SCI & TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211572411.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-11-05
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

The existing biosensors have low mechanical strength, poor stability, complex preparation process, and high cost, making it difficult to efficiently detect material changes in sweat.

Method used

Using chitosan and calcium carbonate films, the directional crystallization of calcium carbonate is induced through the mixed configuration of calcium chloride solution, sodium polyacrylate and sodium carbonate solution, forming a hydrophobic layer with hydrophobic properties and a hydrophilic zone with hydrophilic properties. Design microfluidic channels to realize the preparation of high mechanical strength flexible biosensors.

Benefits of technology

The mechanical strength and stability of the biosensor are improved, and the high sensitivity detection of sweat and statistics of sweat volume and sweat rate are achieved, reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115791772B_ABST
    Figure CN115791772B_ABST
Patent Text Reader

Abstract

The invention discloses the preparation and application of a high mechanical strength flexible biosensor, comprising the following steps: applying a chitosan solution on a glass sheet to form a chitosan coating; preparing a mineralizing solution; completely immersing the chitosan in the mineralizing solution to form a calcium carbonate coating; immersing the calcium carbonate coating in a sodium hydroxide solution to remove the film to form a calcium carbonate film; immersing the calcium carbonate film in an octadecyltrichlorosilane solution to form a hydrophobic layer; patterning the hydrophobic layer to form a hydrophobic region and a hydrophilic region at the same time. The present invention uses a calcium carbonate film as a base material, solves the problems of easy damage, poor stability, and low mechanical strength of existing biosensors, increases the detection life of the biosensor, and has a simple manufacturing process, reduces the manufacturing cost, and can simultaneously use colorimetry and fluorescence methods for sensing detection. In addition to multi-component detection, statistics of sweating amount and sweating rate can also be performed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biosensors, and in particular to the preparation and application of a flexible biosensor with high mechanical strength. Background Art

[0002] Non-invasive testing provides a safe, comfortable, and continuously monitored testing method for current medical diagnosis and analysis. Among many body fluids such as tears, urine, saliva, sweat, and nasal fluid, sweat is the easiest and most convenient body fluid to obtain from the human body. The most abundant component in sweat is water, followed by salt ions, a small amount of lactic acid, urea, trace amounts of amino acids, glucose, and a very small amount of cortisol.

[0003] The metabolism of the above substances is closely related to human diseases. The pH of the human body is between weak acid and neutral, which can serve as a barrier for skin protection. Chloride ion is an important marker of cystic fibrosis in the human body. + , K + , Ca 2+ Reflects the normal bioelectric activity of human cells, among which Na + , K + Abnormal content is likely to induce heart disease. In addition, urea, creatinine and other substances characterize the quality of kidney function, so detecting the concentration of various substances in sweat can directly obtain information about human diseases. However, the biosensors made by existing technology have low mechanical strength and low sensitivity, mainly because the material itself has poor stability, and the existing process manufacturing process is complicated and costly, which is not conducive to mass production. Summary of the invention

[0004] The purpose of the present invention is to provide a preparation and application of a high mechanical strength flexible biosensor to solve the problems of low mechanical strength, poor stability, complex preparation process and high cost of the above-mentioned biosensors used for detecting sweat.

[0005] To achieve the above object, the present invention provides a preparation method of a flexible biosensor with high mechanical strength, comprising the following steps:

[0006] (1) using chitosan solution as a precursor and applying it on a glass sheet to form a chitosan coating;

[0007] (2) preparing a mineralizing solution by mixing a calcium chloride solution, a sodium polyacrylate solution and a sodium carbonate solution;

[0008] (3) completely immersing the chitosan coating in a mineralizing solution to induce directional crystallization of calcium carbonate to form a calcium carbonate coating;

[0009] (4) immersing the calcium carbonate coating in a sodium hydroxide solution to remove the coating and form a calcium carbonate film;

[0010] (5) immersing the calcium carbonate film in an octadecyltrichlorosilane solution to form a hydrophobic layer having a hydrophobic property;

[0011] (6) The hydrophobic layer is patterned to simultaneously form a hydrophobic region with hydrophobic properties and a hydrophilic region with hydrophilic properties, thereby forming a flexible biosensor with high mechanical strength.

[0012] Preferably, the chitosan solution in step (1) is prepared by adding chitosan and glacial acetic acid solution into ultrapure water, stirring and filtering to obtain a chitosan solution, which is stored at below 4° C. for later use, wherein the mass volume ratio of chitosan to glacial acetic acid is 1 g:1 mL.

[0013] Preferably, in step (1), the chitosan solution is coated on the glass sheet, and then heated, dried, immersed in a sodium hydroxide solution, rinsed with deionized water, and dried to obtain the chitosan coating.

[0014] Preferably, the mineralizing liquid in step (2) is prepared by adding anhydrous calcium chloride to ultrapure water and stirring, and then adding sodium polyacrylate and stirring; taking ultrapure water and adding anhydrous sodium carbonate and stirring; adding sodium carbonate solution to calcium chloride and sodium polyacrylate to form a mixed solution, stirring, and filtering to obtain the mineralizing liquid.

[0015] Preferably, in step (3), the glass sheet coated with chitosan is immersed in the mineralizing solution and then placed in a water bath at 25° C. for 6 hours to form a calcium carbonate coating on the surface of the chitosan; in step (4), the dried calcium carbonate coating is immersed in a 0.05 g / mL sodium hydroxide solution for 4 hours, the film is removed, rinsed, immersed in deionized water for 1 hour, rinsed, placed in a culture dish, and naturally dried at room temperature to obtain a calcium carbonate film.

[0016] Preferably, in step (5), the calcium carbonate film is subjected to plasma treatment and then completely immersed in an octadecyltrichlorosilane solution.

[0017] Preferably, in step (6), the surface of the hydrophobic layer is covered with a mask, clamped with a clamp, and treated with ultraviolet light to form a hydrophilic circular hole area and a hydrophilic microfluidic channel.

[0018] The application of the high mechanical strength flexible biosensor obtained by the preparation method, the hydrophilic region is used to enrich sweat, and the hydrophilic region is modified with a colorimetric reagent to realize visual detection of sweat.

[0019] In the application of the high mechanical strength flexible biosensor obtained by the preparation method, the hydrophilic region is used to enrich sample analytes, and the hydrophilic region is modified with fluorescent probes to realize fluorescent detection of sample analytes.

[0020] The high mechanical strength flexible biosensor obtained by the preparation method is applied, and water-active dye is added into the microfluidic channel to realize the calculation of sweating amount and sweating rate.

[0021] Therefore, the preparation and application of a high mechanical strength flexible biosensor using the above structure in the present invention has the following beneficial effects:

[0022] (1) The present invention uses a calcium carbonate film to make a biosensor. Specifically, a calcium chloride solution and a sodium carbonate solution are reacted to generate amorphous calcium carbonate. Under the action of charged polymer sodium polyacrylate, calcium carbonate is induced to crystallize in an oriented manner to generate a calcium carbonate film on the surface of chitosan. The calcium carbonate film itself has extremely high mechanical strength. Bending and friction and wear will not cause changes in the surface morphology and properties. Therefore, the biosensor made using the calcium carbonate film has extremely strong stability. The problems of the existing biosensors being easy to damage, having poor stability, and having low mechanical strength are solved, and the detection life of the biosensor is increased.

[0023] (2) The present invention uses chitosan as the substrate, which has excellent biological functions such as biocompatibility and degradability.

[0024] (3) The present invention achieves two different properties, hydrophobicity and hydrophilicity, on the same interface by surface modification, patterning and then surface functionalization of the calcium carbonate film. By modifying the colorimetric reagent or fluorescent probe, the purpose of constructing a sensing detection area is achieved, thereby realizing high-sensitivity detection of sweat; and the statistics of sweating amount and sweating rate are realized through the designed microfluidic channel.

[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is an electron microscope image of the surface-modified calcium carbonate film;

[0027] Figure 2 This is a contact angle representation diagram of hydrophobic calcium carbonate film;

[0028] Figure 3 This is a contact angle representation diagram of hydrophilic calcium carbonate film;

[0029] Figure 4 This is a physical simulation diagram of a flexible biosensor;

[0030] Figure 5 This is an electron microscope image of a calcium carbonate film after bending and friction wear;

[0031] Figure 6 This is a characterization diagram of the contact angle of the modified calcium carbonate film friction and wear experiment;

[0032] Figure 7 It is the L*a*b* model of sensor visual detection of glucose;

[0033] Figure 8 It is the L*a*b* model of sensor visual detection of pH;

[0034] Fig. 9 It is a curve diagram showing the relationship between the fluorescence intensity detected by the sensor and the change in sample concentration. DETAILED DESCRIPTION

[0035] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.

[0036] Example 1

[0037] A preparation method of a flexible biosensor with high mechanical strength comprises the following steps:

[0038] Step 1: Prepare chitosan solution: add 1 g chitosan and 1 mL glacial acetic acid into 100 mL ultrapure water, stir magnetically for 2 h, filter, and store at 4 degrees Celsius.

[0039] Step 2: Prepare chitosan coating: Use 3M tape to stick the four sides of a clean glass slide, apply 1 mL of chitosan solution, heat on a heating table at 80°C, and after drying, immerse in 0.08 g / mL NaOH solution for 2 min, rinse with deionized water, and dry for later use.

[0040] Step 3: Preparation of mineralizing solution: add 0.0555 g of anhydrous calcium chloride to 50 mL of ultrapure water, stir magnetically for 15 min, then add 0.002 g of sodium polyacrylate, and stir magnetically for 15 min; take another 50 mL of ultrapure water, add 0.053 g of anhydrous sodium carbonate, stir magnetically for 15 min, then add the sodium carbonate solution to the mixed solution of calcium chloride and sodium polyacrylate, stir magnetically for 15 min and filter to form a mineralizing solution.

[0041] Step 4: Preparation of calcium carbonate film: The chitosan coating was completely immersed in the mineralizing solution and sealed, and placed in a water bath at 25 degrees Celsius for 6 hours to induce directional crystallization of calcium carbonate and form a calcium carbonate coating on the surface of the chitosan coating; the dried calcium carbonate coating was immersed in a 0.05g / mL NaOH solution for 3 hours, the film was removed, rinsed, immersed in deionized water for 1 hour, rinsed, placed in a culture dish, and dried naturally at room temperature to obtain a calcium carbonate film.

[0042] Step 5: Surface modification of calcium carbonate film: The calcium carbonate film was treated with a UV plasma cleaner for 6 minutes to clean the surface. Then the sample was completely immersed in 100 μL of octadecyltrichlorosilane solution (10 mL of toluene), sealed and light-proofed, and allowed to stand for half an hour. Then, it was rinsed with anhydrous ethanol to obtain a surface-modified calcium carbonate film (its microscopic morphology is shown in FIG. Figure 1As shown), the surface has a hydrophobic property, forming a hydrophobic layer (as shown Figure 2 shown).

[0043] Step 6: Patterning: Cover the surface of the modified calcium carbonate film (i.e., the hydrophobic layer) with a mask plate, clamp it with a clamp, and after UV treatment for 15min, form a hydrophilic (e.g., Figure 3 The circular hole area and microfluidic channel (as shown in Figure 4 shown).

[0044] Figure 1 This is an electron microscope image of the microscopic morphology of the calcium carbonate film after surface modification. It can be seen from the image that the calcium carbonate film presents an irregular, tightly and continuously arranged polygonal structure. This is the result of inducing directional crystallization of the calcium carbonate solution under the action of sodium polyacrylate. Figure 2 This is a characterization diagram of the surface properties of the modified calcium carbonate film. The contact angle is 121.2±4.9°. The surface-modified calcium carbonate film has hydrophobic properties. Figure 3 This is a characterization diagram of the surface properties of the UV-treated calcium carbonate film. It can be seen from the figure that the contact angle is 9.1±1.5°, and the surface has hydrophilic properties. Figure 4 This is a physical simulation diagram of a flexible biosensor based on calcium carbonate film, which includes a hydrophilic circular pore area on the hydrophobic surface and a hydrophilic microfluidic channel.

[0045] Example 2

[0046] The mechanical strength and surface properties of calcium carbonate films were characterized.

[0047] Take the calcium carbonate film after surface modification (its surface microstructure is as follows Figure 1 As shown), bending and sand were used to perform friction and wear tests on the surface, and the morphology was observed using electron microscope photos (as shown Figure 5 ) did not change significantly, maintaining good mechanical strength. The optical contact angle tension tester was used to analyze the surface properties of the films subjected to different friction and wear times, such as Figure 6 As shown in the figure, the contact angle statistics of the friction and wear surface show that after multiple friction and wear, the surface contact angle has not changed significantly, and the calcium carbonate film can still maintain its hydrophobic state. This shows that the calcium carbonate film has stable surface properties.

[0048] Example 3

[0049] Glucose detection: Prepare sweat standard solutions with glucose concentrations of 1.25, 2.50, 3.75, and 5 mM, respectively. Add 2 μL of glucose colorimetric reagent prepared with enzyme reagent and phenol reagent in a ratio of 1:1 to the hydrophilic circular hole area for functional modification. After drying, add 2 μL of glucose standard solutions of different concentrations respectively. After reaction enrichment, use a smartphone to shoot, record and extract colorimetric reaction information, and establish an L*a*b* model for glucose, where L * The value indicates the brightness change, a * Indicates the change from green to red, b * Indicates a change from yellow to blue. Figure 7 As shown, L * The value gradually decreases with the increase of glucose concentration, the brightness gradually darkens, and the color change gradually deepens, showing good sensitivity, with an error limit between 2-4 and good stability. This shows the feasibility of biosensors for sweat glucose detection.

[0050] Example 4

[0051] pH detection: 2 μL of litmus reagent was added to the hydrophilic circular hole area to achieve functional modification. After drying, the sweat standard solutions with pH values ​​of 6.0, 6.5, 7.0, 7.5, and 8.0 were measured. After reaction enrichment, the colorimetric reaction information was captured and recorded with a smartphone to establish an L*a*b* model for pH value. In this experiment, litmus reagent displays red in the acidic range (6-7) and blue in the alkaline range (7-8). Figure 8 As shown, in the process from acidic to neutral, the brightness gradually increases and the color gradually becomes lighter; in the process from neutral to alkaline, the brightness gradually decreases and the color gradually deepens, showing the feasibility of biosensors for sweat pH detection.

[0052] Example 5

[0053] Preparation 10 -15 , 10 -12 , 10 -9 , 10 -6 , 10 -4 g / mL FITC (fluorescein isothiocyanate) solution, modify FITC (2μL) fluorescent probe in the hydrophilic circular hole area, take pictures with a fluorescence microscope, and establish the relationship curve between fluorescence intensity and sample concentration, such as Fig. 9 As shown, the fluorescence intensity increases with the increase of sample concentration, demonstrating the feasibility of the biosensor for fluorescence detection of analytes.

[0054] Example 6

[0055] A water-active dye CoCl2 is added to the hydrophilic microfluidic channel. It is blue in the anhydrous state and turns red when hydrated (CoCl2 6H2O). After the sweat enters the channel, the color in the channel will turn red as the sweat flows in. The width of the channel is a, the thickness is b, and the distance that the sweat flows into the channel is l. At this time, the sweat volume V is equal to the product of a, b, and l. The time for sweat collection can be recorded as t, so the sweat rate is the ratio of volume to time. It should be noted that since the channel for sweat volume statistics has only one sweat inlet, it is well sealed and the evaporation of sweat can be ignored.

[0056] By designing microfluidic channels of different sizes for different groups of people, personalized statistics can be performed. Figure 4 This is a physical simulation diagram of the flexible biosensor.

[0057] Therefore, the present invention adopts the preparation and application of a high mechanical strength flexible biosensor with the above structure. The present invention realizes two different properties, hydrophobicity and hydrophilicity, on the same interface by surface modification, patterning and then surface functionalization of the calcium carbonate film. By adding a colorimetric reagent or a fluorescent probe, the purpose of constructing a sensing detection area is achieved, and high-sensitivity detection of sweat or other analytes is achieved; at the same time, the statistics of sweating amount and sweating rate are realized through the designed microfluidic channel.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a flexible biosensor with high mechanical strength, characterized in that: The following steps are involved: (1) using chitosan solution as a precursor and applying it on a glass sheet to form a chitosan coating; (2) preparing a mineralizing solution by mixing a calcium chloride solution, a sodium polyacrylate solution and a sodium carbonate solution; (3) completely immersing the chitosan coating in a mineralizing solution to induce directional crystallization of calcium carbonate to form a calcium carbonate coating; (4) immersing the calcium carbonate coating in a sodium hydroxide solution to remove the coating and form a calcium carbonate film; (5) immersing the calcium carbonate film in an octadecyltrichlorosilane solution to form a hydrophobic layer having a hydrophobic property; (6) The hydrophobic layer is patterned to simultaneously form a hydrophobic region with hydrophobic properties and a hydrophilic region with hydrophilic properties, thereby forming a flexible biosensor with high mechanical strength.

2. The method for preparing a high mechanical strength flexible biosensor according to claim 1, characterized in that: The chitosan solution in step (1) is prepared by adding chitosan and glacial acetic acid solution into ultrapure water, stirring and filtering to obtain a chitosan solution, which is stored at below 4° C. for later use, wherein the mass volume ratio of chitosan to glacial acetic acid is 1 g:1 mL.

3. The method for preparing a flexible biosensor with high mechanical strength according to claim 1, characterized in that: In step (1), the chitosan solution is coated on the glass sheet, and then heated, dried, immersed in a sodium hydroxide solution, rinsed with deionized water, and dried to obtain a chitosan coating.

4. The method for preparing a flexible biosensor with high mechanical strength according to claim 1, characterized in that: The mineralizing liquid in step (2) is prepared by adding anhydrous calcium chloride to ultrapure water and stirring, and then adding sodium polyacrylate and stirring; taking ultrapure water and adding anhydrous sodium carbonate and stirring; adding sodium carbonate solution to calcium chloride and sodium polyacrylate to form a mixed solution, stirring and filtering to obtain the mineralizing liquid.

5. The method for preparing a flexible biosensor with high mechanical strength according to claim 1, characterized in that: In step (3), the glass sheet coated with chitosan is immersed in the mineralizing solution and then placed in a water bath at 25° C. for 6 hours to form a calcium carbonate coating on the surface of the chitosan; in step (4), the dried calcium carbonate coating is immersed in a 0.05 g / mL sodium hydroxide solution for 4 hours, the film is removed, rinsed, immersed in deionized water for 1 hour, rinsed, placed in a culture dish, and naturally dried at room temperature to obtain a calcium carbonate film.

6. The method for preparing a flexible biosensor with high mechanical strength according to claim 1, characterized in that: In step (5), the calcium carbonate film is subjected to plasma treatment and then completely immersed in an octadecyltrichlorosilane solution.

7. The method for preparing a flexible biosensor with high mechanical strength according to claim 1, characterized in that: In step (6), the surface of the hydrophobic layer is covered with a mask plate and clamped with a clamp, and after ultraviolet light treatment, a hydrophilic circular hole area and a hydrophilic microfluidic channel are formed.

8. Application of the high mechanical strength flexible biosensor obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The hydrophilic region is used to enrich sweat, and the hydrophilic region is modified with a colorimetric reagent to achieve visual detection of sweat.

9. Application of the high mechanical strength flexible biosensor obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The hydrophilic region is used to enrich sample analytes, and the hydrophilic region is modified with fluorescent probes to achieve fluorescent detection of the analytes.

10. Application of the high mechanical strength flexible biosensor obtained by the preparation method according to claim 7, characterized in that: Water-active dyes were added to the microfluidic channels to measure sweating amount and sweating rate.