A highly stable quantum dot diffusion plate and preparation method thereof

By mixing quantum dot solution and precursor solution with blank masterbatch in an extrusion molding machine to generate a coating layer, the problems of complex preparation and poor stability of quantum dot diffusion plates are solved, and a quantum dot diffusion plate with high stability and low cost is realized.

CN115806712BActive Publication Date: 2024-11-26MINDU INNOVATION LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211379305.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-11-26
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

The existing quantum dot diffuser plate has a complex manufacturing process, making mass production difficult. In addition, quantum dots have poor stability and are easily corroded by water and oxygen in the air, which increases manufacturing costs.

Method used

A quantum dot diffusion plate with a single-layer structure is formed by adding quantum dot solution and quantum dot-coated precursor solution from different feed ports through an extrusion molding machine. These solutions are then mixed with blank masterbatch, dispersant, and additives. The water in the masterbatch is used to carry out a hydrolysis and condensation reaction to generate a coating layer, thus forming a highly stable quantum dot diffusion plate.

Benefits of technology

It simplifies the preparation process, reduces costs, eliminates the need for expensive water and oxygen barrier membranes, improves the stability of quantum dots, and reduces the introduction of impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115806712B_ABST
    Figure CN115806712B_ABST
Patent Text Reader

Abstract

The present invention discloses a highly stable quantum dot diffusion plate and a preparation method thereof, wherein the quantum dot diffusion plate is a single-layer structure, and comprises a quantum dot composite material, a blank masterbatch, a diffusant and an additive; the preparation method comprises: 1. preparing a quantum dot solution; 2. preparing a precursor solution required for coating quantum dots; 3. adding the blank masterbatch, the diffusant and the additive into an extruder from a first feed port, injecting the quantum dot solution and the precursor solution required for coating quantum dots into the extruder from a second feed port, and mixing them evenly with the blank masterbatch, the diffusant and the additive, and then extruding to obtain a highly stable quantum dot diffusion plate. The present invention utilizes the water contained in the blank masterbatch to participate in the reaction of the precursor solution required for coating quantum dots, and forms a quantum dot composite material in the extruder to protect the quantum dots; on the other hand, by reducing the time of the quantum dots in a high temperature environment, the stability of the quantum dots is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of optoelectronic display technology, and in particular to a highly stable quantum dot diffusion plate and a preparation method thereof. Technical Background

[0002] As an important component of the backlight module, the main function of the light diffuser is to fully scatter the incident light to achieve a softer and more uniform light output effect. With the continuous development of display and lighting technology, excellent light diffusers must not only meet the requirements of high light dispersion, softness, and uniform color temperature, but also reduce the harm of blue light, improve the color gamut of transmitted light, and achieve a better match with natural light based on LED as the light source. Therefore, quantum dot diffuser technology came into being, using semiconductor quantum dots with special structures to convert the original blue LED backlight into a purer three-primary color composite white light to improve the color gamut range of the LCD screen.

[0003] The existing patent (application number: 201710378860.2) discloses a process for making a quantum dot diffusion plate and a diffusion plate, which mixes quantum dots with methyl methacrylate with a solvent to form a QD-MMA solution, which is then dried, prepolymerized, molded, baked, and then a water-oxygen barrier film is prepared. The entire process is complicated and difficult to achieve mass production. In addition, it also requires expensive water- and oxygen-isolating films, which invisibly increases the manufacturing cost.

[0004] The existing patent (application number: 202010198836.2) discloses a quantum dot light-emitting functional plate and its preparation method, which first prepares the anion and cation precursors of the synthesized quantum dots separately, then mixes the cation precursor with the diffusant, plastic particles and additives, and finally mixes it with the anion precursor and extrude it to form a quantum dot diffusion plate. This method makes it difficult to remove excess impurities in the quantum dot synthesis process, it is difficult to control the growth structure of the quantum dots, and the grown quantum dots are directly embedded in the diffusion plate substrate. In the absence of an external protective layer, the quantum dots are easily corroded by water and oxygen infiltrating the air, thereby affecting the stability of the quantum dots. Summary of the invention

[0005] The purpose of the present invention is to provide a highly stable quantum dot diffusion plate and a preparation method thereof, which can solve the stability problem of quantum dots in the diffusion plate, and has a simple preparation process, does not require expensive water-proof and oxygen-proof films, and does not introduce unnecessary impurities.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A highly stable quantum dot diffusion plate and a preparation method thereof. The quantum dot diffusion plate is a single-layer structure and comprises, by weight, 100 parts of a blank masterbatch, 0.025-0.15 parts of a quantum dot composite material, 0.01-0.05 parts of a diffusant and 0.01-0.05 parts of an additive. The preparation method comprises: (1) preparing a quantum dot solution; (2) preparing a precursor solution required for coating the quantum dots; (3) adding the blank masterbatch, the diffusant and the additive to an extruder from a first solid feed inlet, injecting the prepared quantum dot solution and the precursor solution required for coating the quantum dots into the extruder from a second liquid feed inlet and mixing them uniformly with the blank masterbatch, the diffusant and the additive, and then contacting the quantum dots with the precursor solution required for coating the quantum dots and performing a hydrolysis condensation reaction under the action of water contained in the blank masterbatch to generate a coating layer, and then extruding and molding the plate through an extruder to form the highly stable quantum dot diffusion plate.

[0008] Furthermore, the quantum dots in the quantum dot solution are alloyed quantum dots with a core-shell structure composed of one or more of group IIB-VIA compounds, group IIIA-VA compounds; the solvent in the quantum dot solution is one or more of a high boiling point solvent such as an ester solvent, an aliphatic hydrocarbon solvent, and an aromatic hydrocarbon solvent; the quantum dot solution can also be a perovskite quantum dot precursor solution.

[0009] Furthermore, the precursor solution required for coating the quantum dots comprises one or more of ethyl orthosilicate, methyl orthosilicate, bis-[3-(triethoxysilyl)-propyl]-tetrasulfide, bis-[3-(triethoxysilyl)-propyl]-disulfide, 3-mercaptopropyl(dimethoxy)silane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, titanium isopropoxide, tetraethyl titanate, aluminum isopropoxide, etc., and also comprises one or more of the catalysts required for the reaction, such as tetramethylammonium hydroxide, dimethylaminoethyl acrylate, and ammonium hydroxide.

[0010] Furthermore, the blank masterbatch can be one or more of polystyrene, polyvinyl chloride, polymethyl methacrylate, polypropylene, a copolymer of ethylene and butylene, a copolymer of ethylene and vinyl acetate, a methyl methacrylate-styrene copolymer, and an acrylonitrile-butadiene-styrene copolymer.

[0011] Furthermore, the diffusant is an inorganic diffusant or an organic diffusant, wherein the inorganic diffusant includes one or more of barium sulfate, calcium carbonate, silicon dioxide, and titanium dioxide, and the organic diffusant includes one or more of acrylic type, styrene type, and acrylic resin type.

[0012] Furthermore, the additives include one or more of an antioxidant, an inhibitor, an antistatic agent, and a toughening agent.

[0013] Furthermore, the antioxidant may be an aromatic amine antioxidant such as diphenylamine, p-phenylenediamine, dihydroxyquinoline and other compounds and their derivatives, or a hindered phenol antioxidant such as 2,6-tert-butyl-4-methylphenol, bis(3,5-tert-butyl-4-hydroxyphenyl)sulfide, tetrakis(β-(3,5-tert-butyl-4-hydroxyphenyl)propionate)pentaerythritol, etc., or an auxiliary antioxidant such as thiodipropionic acid diester, didodecanol ester, didetradecyl alcohol ester and didedecyl alcohol ester, etc., one or more thereof.

[0014] Furthermore, the antistatic agent can be a cationic antistatic agent such as a long-chain alkyl quaternary ammonium, phosphonium or phosphonium salt, an anionic antistatic agent such as an alkali metal salt of alkyl sulfonic acid, phosphoric acid or dithiocarbamic acid, or a nonionic antistatic agent such as ethoxylated aliphatic alkylamine, ethoxylated alkyl acid amine, etc.

[0015] Furthermore, the toughening agent can be one or more of styrene-butadiene thermoplastic elastomer, methyl methacrylate-butadiene-styrene terpolymer, acrylonitrile-butadiene-styrene copolymer, chlorinated polyethylene, ethylene-vinyl acetate copolymer, ethylene-butene copolymer, and ethylene-octene copolymer.

[0016] Furthermore, the extrusion molding conditions in step (3) are: inert environment, molding temperature of 180-260° C., extruder screw speed of 120-200 rpm / min, feeder speed of 5-12 rpm / min, and the thickness of the quantum dot diffusion plate is 0.5-2 mm.

[0017] The beneficial effects of the present invention are:

[0018] The present invention provides a highly stable quantum dot diffusion plate and a preparation method thereof. Compared with the prior art, the quantum dot diffusion plate has the outstanding substantial feature that, during the preparation process of the quantum dot diffusion plate of the present invention, the precursor solution required for coating quantum dots and the quantum dot solution, blank masterbatch, diffusant and additive are respectively added into an extrusion molding machine from different feed ports, and the moisture in the blank masterbatch is used to hydrolyze and condense the precursor solution for coating quantum dots to form a coating layer on the surface of the quantum dots, thereby improving the stability of the quantum dots. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0020] Figure 1 This is a flow chart of a highly stable quantum dot diffusion plate and a preparation method thereof of the present invention;

[0021] Figure 2 1 is a structural schematic diagram of an extrusion molding machine used in a highly stable quantum dot diffusion plate and a preparation method thereof of the present invention, wherein 1 is a first feed inlet: a solid feed inlet, 2 is a feed screw, 3 is an extruder screw, 4 is a heating temperature zone, 5 is a second feed inlet: a liquid feed inlet, 6 is a vacuum port, 7 is an extrusion port, 8 is a quantum dot diffusion plate, 9 is a cooling zone, and 10 is a cutting zone;

[0022] Figure 3 This is a spectrum diagram of a highly stable red quantum dot diffusion plate of the present invention under the excitation of a blue light backlight source;

[0023] Figure 4 This is a spectrum diagram of a highly stable green quantum dot diffusion plate of the present invention under the excitation of a blue light backlight source;

[0024] Figure 5 This is a spectrum diagram of a highly stable yellow quantum dot diffusion plate of the present invention under the excitation of a blue light backlight source;

[0025] Figure 6 This is the test result of a highly stable quantum dot diffusion plate of the present invention under high temperature and high humidity blue light aging;

[0026] Figure 7 It is a performance comparison diagram of quantum dot diffusion plates prepared by feeding from the same feed inlet and different feed inlets of the present invention. DETAILED DESCRIPTION

[0027] The following is a detailed description of a highly stable quantum dot diffusion plate and a preparation method thereof provided by the present invention in conjunction with an embodiment. The present invention provides preferred embodiments, which are only used to further illustrate the present invention and should not be considered to be limited to the embodiments described herein, nor should they be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by persons skilled in the art based on the above invention content still fall within the scope of protection of the present invention.

[0028] Example 1

[0029] This embodiment provides a method for preparing a red quantum dot diffusion plate, and the specific steps are as follows:

[0030] 1. Prepare quantum dot solution: Take 0.025g CdSe / CdS / CdZnS red quantum dots (purchased from Guangdong Pujiafu Optoelectronics Technology Co., Ltd.) and disperse them in 3mL dodecane solvent.

[0031] 2. Prepare the precursor solution required for coating quantum dots: Take 15 mL of ethyl orthosilicate and 2 mL of tetramethylammonium hydroxide and mix them evenly in a syringe to obtain a colorless and transparent precursor solution required for coating quantum dots.

[0032] 3. Adding materials: Add the above-prepared quantum dot solution, the precursor solution required for coating quantum dots, the blank masterbatch, the diffusant and the additive from different feeding ports. Among them, the blank masterbatch, the diffusant and the additive are added from the first solid feed port, and the quantum dot solution and the precursor solution required for coating quantum dots are added from the second liquid feed port. The proportions of each component are: 100 parts of PS, 0.025 parts of CdSe / CdS / CdZnS red quantum dots, 0.025 parts of the precursor solution required for coating quantum dots, 0.025 parts of the diffusant silica and 0.025 parts of the additive antioxidant 168 (purchased from Aladdin Reagent Co., Ltd.).

[0033] 4. Heating: Adjust the temperature control interface to the working temperature, heat the barrel and die head. The extruder is divided into eight temperature zones. The temperature of barrel zone 1 is 190℃, the temperature of barrel zones 2 and 3 is 220℃, the temperature of barrel zones 4-8 is 225℃, and the temperature of die head zone is 225℃. The extruder is equipped with a vacuum exhaust device, and the vacuum degree is controlled at -0.08~-0.1Mpa.

[0034] 5. Extrusion of sheet: Put the evenly mixed blank masterbatch, diffusant and additive into the first feed port, turn on the extruder, feeder and vacuum pump in turn, set the extruder screw speed and feeder speed and other parameters, so that the blank masterbatch passes through the barrel and melts. When the mixture passes through the second feed port, the quantum dot solution and the precursor solution required for coating the quantum dots are injected from the second feed port, mixed with the blank masterbatch, diffusant and additives, the precursor solution required for coating the quantum dots contacts the quantum dots and undergoes hydrolysis and condensation reaction under the action of water in the blank masterbatch to form a coating layer, and then mixed evenly with the molten blank masterbatch and extruded. The reaction solvent is removed by a vacuum pump, and the extruded sheet passes through a roller with a microstructure to hot-press the upper and lower surfaces of the sheet into a specific microstructure.

[0035] 6. Dust removal, cooling and traction: According to production requirements, adjust the width and thickness of the plate with a knife. The thickness of the plate is 1.6mm. After the plate is trimmed, dust is removed and gradually transported to the back end of the production line through a conveyor. During traction, it is gradually cooled and shaped to form a red quantum dot diffusion plate. Figure 3 It is a spectrum diagram of a highly stable red quantum dot diffusion plate of the present invention under the excitation of a blue light backlight source.

[0036] Example 2

[0037] This embodiment provides a method for preparing a green quantum dot diffusion plate, and the specific steps are as follows:

[0038] 1. Prepare quantum dot solution: Take 0.1 g CdZnSeS / ZnS green quantum dots (purchased from Guangdong Pujiafu Optoelectronics Technology Co., Ltd.) and disperse them in 3 mL dodecane solvent.

[0039] 2. Prepare the precursor solution required for coating quantum dots: Take 15 mL of ethyl orthosilicate and 2 mL of tetramethylammonium hydroxide and mix them evenly in a syringe to obtain a colorless and transparent precursor solution required for coating quantum dots.

[0040] 3. Adding materials: Add the above-prepared quantum dot solution, the precursor solution required for coating quantum dots, the blank masterbatch, the diffusant and the additive from different feeding ports. Among them, the blank masterbatch, the diffusant and the additive are added from the first solid feed port, and the quantum dot solution and the precursor solution required for coating quantum dots are added from the second liquid feed port. The proportions of each component are: 100 parts of PS, 0.1 parts of CdZnSeS / ZnS green quantum dots, 0.1 parts of the precursor solution required for coating quantum dots, 0.03 parts of the diffusant silica and 0.02 parts of the additive antioxidant 168 (purchased from Aladdin Reagent Co., Ltd.).

[0041] 4. Heating: Adjust the temperature control interface to the working temperature, heat the barrel and die head. The extruder is divided into eight temperature zones. The temperature of barrel zone 1 is 180℃, the temperature of barrel zones 2 and 3 is 190℃, the temperature of barrel zones 4 and 5 is 200℃, the temperature of barrel zones 6 and 7 is 205℃, the temperature of barrel zone 8 is 210℃, and the temperature of die head zone is 215℃. The extruder is equipped with a vacuum exhaust device, and the vacuum degree is controlled at -0.08~-0.1Mpa.

[0042] 5. Extrusion of sheet: Put the evenly mixed blank masterbatch, diffusant and additive into the first feed port, turn on the extruder, feeder and vacuum pump in turn, set the extruder screw speed and feeder speed and other parameters, so that the blank masterbatch passes through the barrel and melts. When the mixture passes through the second feed port, the quantum dot solution and the precursor solution required for coating the quantum dots are injected from the second feed port, mixed with the blank masterbatch, diffusant and additives, the precursor solution required for coating the quantum dots contacts the quantum dots and undergoes hydrolysis and condensation reaction under the action of water in the blank masterbatch to form a coating layer, and then mixed evenly with the molten blank masterbatch and extruded. The reaction solvent is removed by a vacuum pump, and the extruded sheet passes through a roller with a microstructure to hot-press the upper and lower surfaces of the sheet into a specific microstructure.

[0043] 6. Dust removal, cooling and traction: According to production requirements, adjust the width and thickness of the plate with a knife. The thickness of the plate is 1.6mm. After the plate is trimmed, dust is removed and gradually transported to the back end of the production line through a conveyor. During traction, it is gradually cooled and shaped to form a green quantum dot diffusion plate. Figure 4 It is a spectrum diagram of a highly stable green quantum dot diffusion plate of the present invention under the excitation of a blue light backlight source.

[0044] Example 3

[0045] This embodiment provides a method for preparing a yellow quantum dot diffusion plate, and the specific steps are as follows:

[0046] 1. Prepare quantum dot solution: Disperse 0.025 g of CdSe / CdS / CdZnS red quantum dots and 0.1 g of CdZnSeS / ZnS green quantum dots in 3 mL of dodecane solvent respectively.

[0047] 2. Prepare the precursor solution required for coating quantum dots: Take 15 mL of ethyl orthosilicate and 2 mL of tetramethylammonium hydroxide and mix them evenly in a syringe to obtain a colorless and transparent precursor solution required for coating quantum dots.

[0048] 3. Adding materials: Add the above-prepared quantum dot solution, the precursor solution required for coating quantum dots, the blank masterbatch, the diffusant and the additive from different feeding ports. Among them, the blank masterbatch, the diffusant and the additive are added from the first solid feed port, and the quantum dot solution and the precursor solution required for coating quantum dots are added from the second liquid feed port. The proportions of each component are: 100 parts of PS, 0.025 parts of CdSe / CdS / CdZnS red quantum dots, 0.1 parts of CdZnSeS / ZnS green quantum dots, 0.02 parts of the precursor solution required for coating quantum dots, 0.05 parts of the diffusant silica and 0.05 parts of the additive antioxidant 168.

[0049] 4. Heating: Adjust the temperature control interface to the working temperature, heat the barrel and die head. The extruder is divided into eight temperature zones. The temperature of barrel zone 1 is 190℃, the temperature of barrel zones 2 and 3 is 220℃, the temperature of barrel zones 4-8 is 225℃, and the temperature of die head zone is 225℃. The extruder is equipped with a vacuum exhaust device, and the vacuum degree is controlled at -0.08~-0.1Mpa.

[0050] 5. Extrusion of sheet: Put the evenly mixed blank masterbatch, diffusant and additive into the first feed port, turn on the extruder, feeder and vacuum pump in turn, set the extruder screw speed and feeder speed and other parameters, so that the blank masterbatch passes through the barrel and melts. When the mixture passes through the second feed port, the quantum dot solution and the precursor solution required for coating the quantum dots are injected from the second feed port, mixed with the blank masterbatch, diffusant and additives, the precursor solution required for coating the quantum dots contacts the quantum dots and undergoes hydrolysis and condensation reaction under the action of water in the blank masterbatch to form a coating layer, and then mixed evenly with the molten blank masterbatch and extruded. The reaction solvent is removed by a vacuum pump, and the extruded sheet passes through a roller with a microstructure to hot-press the upper and lower surfaces of the sheet into a specific microstructure.

[0051] 6. Dust removal, cooling and traction: According to production requirements, the width and thickness of the plate are adjusted by cutting. The thickness of the plate is 1.6mm. After the plate is trimmed, dust is removed and gradually transported to the back end of the production line through a conveyor. During traction, it is gradually cooled and shaped to form a yellow quantum dot diffusion plate. Figure 5 It is a spectrum diagram of a highly stable yellow quantum dot diffusion plate of the present invention under the excitation of a blue light backlight source. Figure 6 The results are a comparison of the test results of a highly stable quantum dot diffusion plate of the present invention and a common quantum dot diffusion plate under high temperature and high humidity blue light aging. It can be seen that the highly stable quantum dot diffusion plate of the present invention has good stability.

[0052] Example 4

[0053] This example is a comparative example, comparing the performance of quantum dot diffusion plates prepared by feeding from the same feed port and different feed ports. The specific steps are the same as those in Example 1, except that the feeding method in step 3 is to add the prepared quantum dot solution, the precursor solution required for coating the quantum dots, the blank masterbatch, the diffusant and the additive from the first feed port solid feed port, and the remaining steps remain unchanged and will not be repeated here. Figure 7 The performance comparison of quantum dot diffusion plates prepared by two feeding methods shows that the performance of quantum dot diffusion plates prepared by feeding from the same feeding port is nearly 40% lower than that of those prepared by feeding from different feeding ports. This is mainly because feeding from the same feeding port increases the heating time of quantum dots. Quantum dots cannot withstand long-term high temperatures, which leads to their failure. Therefore, feeding from different feeding ports can reduce the heating time of quantum dots and maintain their good performance.

[0054] This patent is not limited to the above-mentioned best implementation mode. Anyone can derive other forms of highly stable quantum dot diffusion plates and preparation methods thereof under the inspiration of this patent. All equivalent changes and modifications made within the scope of the patent of the present invention shall fall within the scope of this patent.

Claims

1. A method for preparing a highly stable quantum dot diffusion plate, characterized in that: The quantum dot diffusion plate is a single-layer structure, and the preparation method comprises the following steps: (1) Preparing quantum dot solution; (2) preparing a precursor solution required for coating quantum dots, wherein the precursor solution comprises one or more of ethyl orthosilicate, methyl orthosilicate, bis-[3-(triethoxysilyl)-propyl]-tetrasulfide, bis-[3-(triethoxysilyl)-propyl]-disulfide, 3-mercaptopropyl(dimethoxy)silane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane titanium isopropoxide, tetraethyl titanate, and aluminum isopropoxide, and the catalyst required for the reaction is one or more of tetramethylammonium hydroxide, dimethylaminoethyl acrylate, and ammonium hydroxide; (3) Adding blank masterbatch, diffusing agent and additives into the extruder from the first solid feed port, injecting the prepared quantum dot solution and the precursor solution required for coating the quantum dots into the extruder from the second liquid feed port respectively, and mixing them evenly with the blank masterbatch, diffusing agent and additives, the precursor solution required for coating the quantum dots contacts the quantum dots and undergoes a hydrolysis condensation reaction under the action of the water contained in the blank masterbatch to form a coating layer, which is then extruded through the extruder to obtain a highly stable quantum dot diffusion plate.

2. The method for preparing a highly stable quantum dot diffusion plate according to claim 1, characterized in that: The quantum dots in the quantum dot solution are alloyed quantum dots with a core-shell structure composed of one or more of group IIB-VIA compounds and group IIIA-VA compounds; the solvent in the quantum dot solution is one or more of a high-boiling point solvent ester solvent, an aliphatic hydrocarbon solvent, and an aromatic hydrocarbon solvent.

3. The method for preparing a highly stable quantum dot diffusion plate according to claim 1, characterized in that: The quantum dot solution is a perovskite quantum dot precursor solution.

4. The method for preparing a highly stable quantum dot diffusion plate according to claim 1, characterized in that: The blank masterbatch is one or more of polystyrene, polyvinyl chloride, polymethyl methacrylate, polypropylene, copolymer of ethylene and butylene, copolymer of ethylene and vinyl acetate, methyl methacrylate-styrene copolymer, and acrylonitrile-butadiene-styrene copolymer.

5. The method for preparing a highly stable quantum dot diffusion plate according to claim 1, characterized in that: The diffusant is an inorganic diffusant or an organic diffusant, wherein the inorganic diffusant includes one or more of barium sulfate, calcium carbonate, silicon dioxide, and titanium dioxide, and the organic diffusant includes one or more of acrylic type, styrene type, and acrylic resin type.

6. The method for preparing a highly stable quantum dot diffusion plate according to claim 1, characterized in that: The additives include one or more of antioxidants, inhibitors, antistatic agents and toughening agents.

7. The method for preparing a highly stable quantum dot diffusion plate according to claim 6, characterized in that: The antioxidant is an aromatic amine antioxidant or a hindered phenol antioxidant; the antistatic agent is a long-chain alkyl quaternary ammonium, phosphorus or phosphonium salt, an alkali metal salt of alkyl sulfonic acid, phosphoric acid or dithiocarbamic acid, an ethoxylated aliphatic alkylamine or an ethoxylated alkyl acid amine; the toughening agent is one or more of styrene-butadiene thermoplastic elastomer, methyl methacrylate-butadiene-styrene terpolymer, acrylonitrile-butadiene-styrene copolymer, chlorinated polyethylene, ethylene-vinyl acetate copolymer, ethylene-butene copolymer, and ethylene-octene copolymer.

8. The method for preparing a highly stable quantum dot diffusion plate according to claim 1, characterized in that: The extrusion molding conditions in step (3) are: inert environment, molding temperature of 180-260° C., extruder screw speed of 120-200 rpm / min, feeder speed of 5-12 rpm / min, and the thickness of the quantum dot diffusion plate is 0.5-2 mm.

9. A highly stable quantum dot diffusion plate made by the preparation method according to any one of claims 1 to 8.