Polyurethane hot melt adhesive for plate edge sealing and preparation method thereof

By reacting polyester polyol with isocyanate and introducing inorganic powder materials and polyurethane adhesives, the bonding, waterproofing and temperature resistance of polyurethane hot melt adhesive for edge sealing of sheets is improved, and the stability and aesthetics of traditional adhesives are solved. Problem, suitable for various sheet edge seals.

CN115820196BActive Publication Date: 2024-11-22CONFAY ADHESIVE TECH (GUANGDONG) CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211527270.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-22
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

Traditional PUR adhesives have insufficient bonding stability when used in edge sealing of sheets, and the adhesive wires are prone to overflow and affect their aesthetics, and their waterproof and temperature resistance need to be improved.

Method used

Polyurethane hot melt adhesive prepared by reacting polyester polyols A, B, C with isocyanate, combined with 800-1500 mesh inorganic powder material and 300-1200mPa·s polyurethane adhesive, control the mass ratio and reaction conditions to improve bonding, Waterproof and temperature resistance.

Benefits of technology

The prepared polyurethane hot melt adhesive wire is thin, has excellent waterproof and temperature resistance, and has high bonding strength. It is suitable for edge sealing of solid wood, wood plastic, particle board and other boards, reducing the cost of edge sealing glue and ensuring the beauty of finished furniture. Spend.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003973370190000071
    Figure BDA0003973370190000071
Patent Text Reader

Abstract

The invention relates to the technical field of C09J175 / 00, and specifically relates to a polyurethane hot melt adhesive for plate edge sealing and a preparation method thereof. The preparation raw materials thereof at least comprise, by weight, 10-25 parts of polyester polyol A, 10-20 parts of polyester polyol B, 5-20 parts of polyester polyol C, 10-20 parts of inorganic powder material, 10-20 parts of polyurethane adhesive, and 5-15 parts of isocyanate. The polyurethane hot melt adhesive for plate edge sealing has a thin adhesive line, excellent waterproof performance and temperature resistance, high bonding strength, is suitable for edge sealing of plates such as solid wood, wood-plastic, particleboard, medium-density fiberboard, etc., is simple to operate, and is subject to mild conditions, and is suitable for large-scale production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of C09J175 / 00, in particular to a polyurethane hot melt adhesive for plate edge sealing and a preparation method thereof. Background Art

[0002] PUR is the abbreviation of Polyurethane Reactive, which belongs to the polyurethane system. According to chemical properties, polyurethane hot melt adhesive can be divided into two categories, one is thermoplastic polyurethane hot melt adhesive, and the other is reactive polyurethane hot melt adhesive. The former forms a bond by cooling and hardening after heating, while the latter forms a bond by cooling and reacting with moisture to crosslink and harden after heating. Thermoplastic polyurethane hot melt adhesive is also called hot melt polyurethane hot melt adhesive (TPU), while reactive polyurethane hot melt adhesive (PUR) can be divided into moisture-curing polyurethane hot melt adhesive and closed polyurethane hot melt adhesive. The PUR we often talk about is a moisture-curing reactive polyurethane hot melt adhesive. Traditional PUR adhesives have low initial strength, but it takes a long time for chemical reaction to reach the final bonding strength; with the advancement of technology, although PUR adhesives can achieve a complete hardening time of 3 days or even a few hours, and the processing process is more stable and reliable than before, the bonding stability when used as edge banding for solid wood, wood-plastic, particleboard, medium-density fiberboard and other boards needs to be further improved.

[0003] Glue lines are a common problem during the use of edge banding adhesive. Very fine glue overflows at the edges and corners of the board. In addition, the base material has different color depths and textures, and the glue lines will seriously affect the aesthetics of the finished furniture. A Chinese patent application (publication number CN114736644A) discloses a transparent edge banding adhesive and a preparation method thereof. Specifically, polyether polyols and polyester polyols are used as main raw materials, and transparent polyurethane elastomers and copolyesters are used in combination to make the provided edge banding adhesive transparent, reduce the contrast between the glue and the base material, and weaken the effect of the glue lines on the appearance. However, the waterproof performance, temperature resistance and bonding strength need to be further improved. Summary of the invention

[0004] Therefore, in view of the above defects, the present invention provides a polyurethane hot melt adhesive for board edge sealing. The polyurethane hot melt adhesive for board edge sealing has a thin adhesive line, excellent waterproof and heat resistance, and high bonding strength, and is suitable for edge sealing of boards such as solid wood, wood plastic, particleboard, and medium-density fiberboard.

[0005] On the one hand, the present invention provides a polyurethane hot melt adhesive for plate edge sealing. The preparation raw materials thereof include at least, by weight: 10-25 parts of polyester polyol A, 10-20 parts of polyester polyol B, 5-20 parts of polyester polyol C, 10-20 parts of inorganic powder material, 10-20 parts of polyurethane adhesive, and 5-15 parts of isocyanate.

[0006] As a preferred technical solution, the mass ratio of the polyester polyol A, polyester polyol B and polyester polyol C is (15-20): (15-20): (8-18).

[0007] As a preferred technical solution, the polyester polyol A is a crystalline polyester polyol, the hydroxyl value of the crystalline polyester polyol is 27-34 mgKOH / g, and the molecular weight is 3000-4000 g / moL. Preferably, the model of the crystalline polyester polyol is Evonik polyester polyol 7380.

[0008] As a preferred technical solution, the polyester polyol B and polyester polyol C are amorphous polyester polyols; the hydroxyl value of the amorphous polyester polyol is 18-60 mgKOH / g and the molecular weight is 2000-5500 g / moL. Preferably, the hydroxyl value of the polyester polyol B is 31-39 mgKOH / g and the molecular weight is 2500-3500 g / moL. Preferably, the hydroxyl value of the polyester polyol C is 38-46 mgKOH / g and the molecular weight is 2000-3000 g / moL. The model of the polyester polyol B is Evonik polyester polyol 7130, and the model of the polyester polyol C is Evonik polyester polyol 7150.

[0009] Based on the present invention, crystalline polyester polyol A and amorphous polyester polyols B and C are used, and in particular, the mass ratio of the polyester polyol A, polyester polyol B, and polyester polyol C is controlled to be (15-20): (15-20): (8-18). The moisture-curing hot melt adhesive prepared after reacting with the isocyanate in the system has excellent bonding performance, temperature resistance and water resistance, and avoids the problem of rapid shrinkage when cooled.

[0010] As a preferred technical solution, the isocyanate is diphenylmethane diisocyanate and / or polymethylene polyphenyl polyisocyanate.

[0011] As a preferred technical solution, the particle size of the inorganic powder material is 800-1500 mesh. Preferably, the inorganic powder material is at least one of talcum powder, heavy calcium powder, and bentonite; preferably, the inorganic powder material is 1000 mesh talcum powder. Based on the system of the present invention, the introduction of 800-1500 mesh inorganic powder materials, especially the introduction of 1000 mesh talcum powder, effectively reduces the cost of edge banding glue, improves the overall mechanical properties of edge banding glue, and makes the prepared edge banding glue line thin, thereby ensuring the aesthetics of the finished furniture.

[0012] As a preferred technical solution, the viscosity (25°C) of the polyurethane adhesive is 300-1200 mPa·s. Preferably, the viscosity (25°C) of the polyurethane adhesive is 300-600 mPa·s, and the model of the polyurethane adhesive is Covestro DESMOCOLL540 / 1.

[0013] Based on the system of the present invention, a polyurethane adhesive with a viscosity (25°C) of 300-1200 mPa·s, especially a polyurethane adhesive with a viscosity (25°C) of 300-600 mPa·s, is introduced to interact with the polyester polyols A, B, and C in the system in a coordinated manner with the isocyanate to further improve the temperature resistance and waterproof properties of the edge sealing adhesive, improve the cohesive strength and adhesion properties of the edge sealing adhesive, and achieve good bonding with the substrate.

[0014] Another aspect of the present invention provides a method for preparing a polyurethane hot melt adhesive for edge sealing of a plate, comprising at least the following steps:

[0015] S1. Put polyester polyol A, polyester polyol B, polyester polyol C, inorganic powder material and polyurethane adhesive into a reaction kettle in order according to weight, stir them evenly and heat them to 120-150°C to dissolve and dehydrate them;

[0016] S2, then keep the temperature at 120-150°C for 100-150 minutes, reduce the material temperature to 70-90°C, and add isocyanate;

[0017] S3, then control the temperature to 100-110°C and react for 1.5-3h before discharging the material.

[0018] Beneficial Effects

[0019] 1. The present invention provides a polyurethane hot melt adhesive for board edge sealing. The polyurethane hot melt adhesive for board edge sealing has a thin adhesive line, excellent waterproof and heat-resistant properties, and high bonding strength. It is suitable for edge sealing of solid wood, wood-plastic, particleboard, medium-density fiberboard and other boards.

[0020] 2. The preparation method of the polyurethane hot melt adhesive for plate edge sealing provided by the present invention is simple to operate, requires mild conditions, and is suitable for large-scale production and application.

[0021] 3. Based on the system of the present invention, crystalline polyester polyol A and amorphous polyester polyols B and C are used, and in particular, the mass ratio of the polyester polyol A, polyester polyol B, and polyester polyol C is controlled to be (15-20): (15-20): (8-18). The moisture-curing hot melt adhesive prepared after reacting with the isocyanate in the system has excellent bonding performance, temperature resistance and water resistance, and avoids the problem of rapid shrinkage when cooled.

[0022] 4. Based on the system of the present invention, an inorganic powder material with a mesh size of 800-1500 is introduced, especially talcum powder with a mesh size of 1000, which effectively reduces the cost of the edge banding adhesive, improves the overall mechanical properties of the edge banding adhesive, and makes the prepared edge banding adhesive line thin, thereby ensuring the aesthetics of the finished furniture.

[0023] 5. Based on the system of the present invention, a polyurethane adhesive with a viscosity (25°C) of 300-1200 mPa·s, especially a polyurethane adhesive with a viscosity (25°C) of 300-600 mPa·s, is introduced to interact with the polyester polyols A, B, and C in the system in a synergistic manner with the isocyanate to further improve the temperature resistance and waterproof properties of the edge sealing adhesive, improve the cohesive strength and adhesion properties of the edge sealing adhesive, and achieve good bonding with the substrate. DETAILED DESCRIPTION

[0024] Example 1

[0025] Embodiment 1 of the present invention provides a polyurethane hot melt adhesive for edge banding of panels. The raw materials for its preparation include, in parts by weight: 18 parts of polyester polyol A, 18 parts of polyester polyol B, 15 parts of polyester polyol C, 15 parts of inorganic powder material, 15 parts of polyurethane adhesive, and 9 parts of isocyanate.

[0026] The polyester polyol A is a crystalline polyester polyol, the hydroxyl value of the crystalline polyester polyol is 27-34 mgKOH / g, the molecular weight is 3500 g / moL, and the model of the crystalline polyester polyol is Evonik polyester polyol 7380.

[0027] The polyester polyol B and polyester polyol C are amorphous polyester polyols; the hydroxyl value of the polyester polyol B is 31-39 mgKOH / g and the molecular weight is 3000 g / moL. The hydroxyl value of the polyester polyol C is 38-46 mgKOH / g and the molecular weight is 2600 g / moL. The model of the polyester polyol B is Evonik polyester polyol 7130, and the model of the polyester polyol C is Evonik polyester polyol 7150.

[0028] The isocyanate is diphenylmethane diisocyanate.

[0029] The inorganic powder material is 1000 mesh talc.

[0030] The viscosity (25° C.) of the polyurethane adhesive is 300 mPa·s, and the model of the polyurethane adhesive is Covestro DESMOCOLL540 / 1.

[0031] Embodiment 1 of the present invention provides, on the other hand, a method for preparing a polyurethane hot melt adhesive for edge sealing of a plate, comprising the following steps:

[0032] S1. According to parts by weight, polyester polyol A, polyester polyol B, polyester polyol C, inorganic powder material and polyurethane adhesive are put into a reaction kettle in order, stirred evenly and heated to 140°C to dissolve and dehydrate;

[0033] S2, then keep the temperature at 140°C for 120 min, reduce the material temperature to 80°C, and add isocyanate;

[0034] S3, then control the temperature to 105°C and react for 2h before discharging the material.

[0035] Example 2

[0036] Embodiment 2 of the present invention provides a polyurethane hot melt adhesive for edge banding of panels. The raw materials for its preparation include, in parts by weight: 20 parts of polyester polyol A, 20 parts of polyester polyol B, 18 parts of polyester polyol C, 18 parts of inorganic powder material, 20 parts of polyurethane adhesive, and 10 parts of isocyanate.

[0037] The polyester polyol A is a crystalline polyester polyol, the hydroxyl value of the crystalline polyester polyol is 27-34 mgKOH / g, the molecular weight is 3500 g / moL, and the model of the crystalline polyester polyol is Evonik polyester polyol 7380.

[0038] The polyester polyol B and polyester polyol C are amorphous polyester polyols; the hydroxyl value of the polyester polyol B is 31-39 mgKOH / g and the molecular weight is 3000 g / moL. The hydroxyl value of the polyester polyol C is 38-46 mgKOH / g and the molecular weight is 2600 g / moL. The model of the polyester polyol B is Evonik polyester polyol 7130, and the model of the polyester polyol C is Evonik polyester polyol 7150.

[0039] The isocyanate is diphenylmethane diisocyanate.

[0040] The inorganic powder material is 1000 mesh talc.

[0041] The viscosity (25° C.) of the polyurethane adhesive is 300 mPa·s, and the model of the polyurethane adhesive is Covestro DESMOCOLL540 / 1.

[0042] Embodiment 2 of the present invention provides, on the other hand, a method for preparing a polyurethane hot melt adhesive for edge sealing of a plate, comprising the following steps:

[0043] S1. According to parts by weight, polyester polyol A, polyester polyol B, polyester polyol C, inorganic powder material and polyurethane adhesive are put into a reaction kettle in order, stirred evenly and heated to 140°C to dissolve and dehydrate;

[0044] S2, then keep the temperature at 140°C for 120 min, reduce the material temperature to 80°C, and add isocyanate;

[0045] S3, then control the temperature to 105°C and react for 2h before discharging the material.

[0046] Example 3

[0047] Embodiment 3 of the present invention provides a polyurethane hot melt adhesive for edge banding of panels. The raw materials for its preparation include, in parts by weight: 15 parts of polyester polyol A, 15 parts of polyester polyol B, 10 parts of polyester polyol C, 15 parts of inorganic powder material, 10 parts of polyurethane adhesive, and 8 parts of isocyanate.

[0048] The polyester polyol A is a crystalline polyester polyol, the hydroxyl value of the crystalline polyester polyol is 27-34 mgKOH / g, the molecular weight is 3500 g / moL, and the model of the crystalline polyester polyol is Evonik polyester polyol 7380.

[0049] The polyester polyol B and polyester polyol C are amorphous polyester polyols; the hydroxyl value of the polyester polyol B is 31-39 mgKOH / g and the molecular weight is 3000 g / moL. The hydroxyl value of the polyester polyol C is 38-46 mgKOH / g and the molecular weight is 2600 g / moL. The model of the polyester polyol B is Evonik polyester polyol 7130, and the model of the polyester polyol C is Evonik polyester polyol 7150.

[0050] The isocyanate is diphenylmethane diisocyanate.

[0051] The inorganic powder material is 1000 mesh talc.

[0052] The viscosity (25° C.) of the polyurethane adhesive is 300 mPa·s, and the model of the polyurethane adhesive is Covestro DESMOCOLL540 / 1.

[0053] Embodiment 3 of the present invention provides, on the other hand, a method for preparing a polyurethane hot melt adhesive for edge sealing of a plate, comprising the following steps:

[0054] S1. According to parts by weight, polyester polyol A, polyester polyol B, polyester polyol C, inorganic powder material and polyurethane adhesive are put into a reaction kettle in order, stirred evenly and heated to 140°C to dissolve and dehydrate;

[0055] S2, then keep the temperature at 140°C for 120 min, reduce the material temperature to 80°C, and add isocyanate;

[0056] S3, then control the temperature to 105°C and react for 2h before discharging the material.

[0057] Comparative Example 1

[0058] Comparative Example 1 of the present invention provides a polyurethane hot melt adhesive for edge banding of panels, and its specific implementation method is the same as that of Example 1, except that, in parts by weight, its preparation raw materials include: 45 parts of polyester polyol A, 3 parts of polyester polyol B, 3 parts of polyester polyol C, 15 parts of inorganic powder material, 15 parts of polyurethane adhesive, and 9 parts of isocyanate; the mass ratio of the polyester polyol A, polyester polyol B, and polyester polyol C is 45:3:3.

[0059] Comparative Example 2

[0060] Comparative Example 2 of the present invention provides a polyurethane hot melt adhesive for edge sealing of panels, and its specific implementation method is the same as that of Example 1, except that, in parts by weight, its preparation raw materials include: 18 parts of polyester polyol A, 18 parts of polyester polyol B, 15 parts of polyester polyol C, 15 parts of inorganic powder material, and 9 parts of isocyanate.

[0061] Performance Testing Methods

[0062] The performance of the polyurethane hot melt adhesive for edge sealing of plates provided in Examples 1-3 and Comparative Examples 1-2 was tested:

[0063] (1) The 180-degree peeling force was tested according to the test method described in GB / T 7124-2008; the substrate was a fiber density board and the adhesive application area was 10 mm*20 mm. The results are shown in Table 1.

[0064] (2) With fiber density board as the substrate and the adhesive application area of ​​10mm*20mm, the edge-sealed board is placed in 50℃ water and soaked for 12 hours. After 12 hours, it is taken out and observed. If the edge-sealing adhesive does not change after absorbing water, the waterproof performance of the polyurethane hot melt adhesive is recorded as "qualified"; if the edge-sealing adhesive expands after absorbing water, the waterproof performance of the polyurethane hot melt adhesive is recorded as "unqualified".

[0065] (3) With fiber density board as substrate and adhesive application area of ​​10mm*20mm, place the edge-sealed board at 140℃ for 2h, take it out and observe it after 2h. If there is no change in the edge-sealing adhesive, the heat resistance of the polyurethane hot melt adhesive is recorded as "qualified"; if the edge-sealing adhesive layer softens, the heat resistance of the polyurethane hot melt adhesive is recorded as "unqualified".

[0066] Table 1

[0067]

[0068] Note: The above performance tests are carried out after the polyurethane hot melt adhesive is cured at 150°C for 30 minutes.

Claims

1. A polyurethane hot melt adhesive for plate edge sealing, characterized in that: The raw materials for its preparation include at least 10-25 parts of polyester polyol A, 10-20 parts of polyester polyol B, 5-20 parts of polyester polyol C, 10-20 parts of inorganic powder material, 10-20 parts of polyurethane adhesive, and 5-15 parts of isocyanate in parts by weight; the mass ratio of the polyester polyol A, polyester polyol B, and polyester polyol C is (15-20): (15-20): (8-18); the polyester polyol A is Evonik polyester polyol 7 380; the polyester polyol B and polyester polyol C are amorphous polyester polyols; the model of the polyester polyol B is Evonik polyester polyol 7130, and the model of the polyester polyol C is Evonik polyester polyol 7150; the inorganic powder material is 1000 mesh talc; the model of the polyurethane adhesive is Covestro DESMOCOLL540 / 1; the isocyanate is diphenylmethane diisocyanate and / or polymethylene polyphenyl polyisocyanate.

2. A method for preparing a polyurethane hot melt adhesive for plate edge sealing according to claim 1, characterized in that: At least the following steps are included: S1. Put polyester polyol A, polyester polyol B, polyester polyol C, inorganic powder material and polyurethane adhesive into a reaction kettle in order according to weight, stir them evenly and heat them to 120-150°C to dissolve and dehydrate them; S2, then keep the temperature at 120-150°C for 100-150 minutes, reduce the material temperature to 70-90°C, and add isocyanate; S3, then control the temperature to 100-110°C and react for 1.5-3h before discharging the material.

Citation Information

Patent Citations

  • Transparent edge sealing adhesive and preparation method thereof

    CN114736644A

  • Polyurethane hot melt adhesive used for garment interlining and preparation method thereof

    CN107418494A

  • Moisture-curing polyurethane hot melt adhesive for coating special-shaped surfaces of furniture and decorative components

    CN107488430A

  • Reactive polyurethane hot melt adhesive for PVC and preparation method thereof

    CN109777336A

  • High-initial strength reaction-type polyurethane hot melt adhesive and preparation method thereof

    CN110256999A