Conductive thermoplastic vulcanized rubber and preparation method thereof

By using ultrasonic dispersion technology and double granulation process of graphene and paraffin oil in thermoplastic vulcanized rubber, combined with vulcanizing agent and other ingredients, the problems of poor conductivity, slow heat dissipation, low strength and poor rebound performance are solved, and conductive type products are realized. Thermoplastic vulcanized rubber has high conductivity, antistatic, fast heat dissipation and excellent mechanical properties.

CN115850873BActive Publication Date: 2024-10-29NINGBO GONEO PHOTOELECTRIC TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211627007.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-10-29
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

Existing thermoplastic vulcanized rubber has poor electrical conductivity, slow heat dissipation, low strength, and poor resilience.

Method used

Graphene is used as a conductive material. It is ultrasonically dispersed with paraffin oil to form a dispersion, and is granulated twice in a screw extruder. It is combined with vulcanizing agents and other ingredients to improve the conductive properties, antistatic capabilities, and heat dissipation rate of the material. and mechanical properties.

Benefits of technology

It achieves stable and continuous extrusion of conductive thermoplastic vulcanized rubber, improves conductive properties, antistatic capabilities, heat dissipation rate and mechanical properties, and ensures high strength and good resilience of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer materials, and in particular to a conductive thermoplastic vulcanized rubber and a preparation method thereof; the components of the conductive thermoplastic vulcanized rubber include, by weight: 95 to 98 parts of a thermoplastic vulcanized rubber masterbatch; 0.5 to 1.2 parts of a vulcanizing agent; 0.3 to 0.6 parts of a first antioxidant; 0.3 to 0.8 parts of a light stabilizer; 0.2 to 0.5 parts of a lubricant; and 0.2 to 0.5 parts of a first paraffin oil; wherein the thermoplastic vulcanized rubber masterbatch includes graphene. The conductive thermoplastic vulcanized rubber of the present invention can not only be stably and continuously extruded, but also has good conductivity, antistatic properties, fast heat dissipation, high strength, and good resilience.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to conductive thermoplastic vulcanized rubber and a preparation method thereof. Background Art

[0002] Thermoplastic vulcanizate (TPV), also known as thermoplastic dynamic vulcanized rubber, consists of two parts: one is plastic, which serves as a continuous phase, and the other is rubber, which serves as a dispersed phase. Thermoplastic vulcanizate has good processing properties, and its extruded products can be used in wires and cables, extruded pipes, profiles, sealing strips, water cutting, mud troughs, etc.

[0003] However, the thermoplastic vulcanized rubber provided by the related art has poor electrical conductivity, slow heat dissipation, low strength and poor resilience. Summary of the invention

[0004] The object of the present invention is to provide a conductive thermoplastic vulcanized rubber and a preparation method thereof. The conductive thermoplastic vulcanized rubber of the present invention can not only be stably and continuously extruded, but also has good conductivity, antistatic properties, fast heat dissipation, high strength, excellent mechanical properties and good resilience.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a conductive thermoplastic vulcanized rubber. The conductive thermoplastic vulcanized rubber comprises the following components in parts by weight:

[0007] Thermoplastic vulcanized rubber masterbatch 95-98 parts;

[0008] Vulcanizing agent 0.5~1.2 parts;

[0009] 0.3-0.6 parts of the first antioxidant;

[0010] Light stabilizer 0.3~0.8 parts;

[0011] Lubricant 0.2~0.5 parts;

[0012] 0.2-0.5 parts of the first paraffin oil; wherein,

[0013] Thermoplastic vulcanizate masterbatch includes graphene.

[0014] In an optional embodiment, the graphene has a carbon content of 98-99.5wt%, a sheet diameter of 1-10μm, a thickness of 2~3nm, a moisture content of <2Wt%, a D50 particle size of less than or equal to 9μm, and a conductivity of 500~600S / cm.

[0015] In an optional embodiment, the thermoplastic vulcanized rubber masterbatch further includes polypropylene resin, ethylene propylene diene monomer rubber, a second paraffin oil, an inorganic filler, a vulcanizing agent, a second antioxidant, and a masterbatch.

[0016] In an optional embodiment, the thermoplastic vulcanized rubber masterbatch includes, by weight, 10 to 20 parts of polypropylene resin, 25 to 40 parts of EPDM rubber, 20 to 40 parts of a second paraffin oil, 2 to 4 parts of graphene, 5 to 10 parts of an inorganic filler, 1 to 3 parts of a vulcanizing agent, 0.2 to 0.6 parts of a second antioxidant, and 0.5 to 2 parts of a masterbatch.

[0017] In an optional embodiment, the Mooney viscosity of the EPDM rubber is 85-100, the ethylene content is 40-60%, and the content of the third monomer is 4.5-7%.

[0018] In a second aspect, the present invention provides a method for preparing a conductive thermoplastic vulcanizate according to any one of the aforementioned embodiments, comprising:

[0019] preparing a graphene-paraffin oil dispersion;

[0020] The polypropylene resin, EPDM rubber, inorganic filler, vulcanizing agent, second antioxidant and masterbatch are blended, and the blended materials are added into a screw extruder for first melting, and graphene-paraffin oil dispersion is added during the first melting process, and extrusion granulation is performed for the first time to obtain a thermoplastic vulcanized rubber masterbatch;

[0021] The thermoplastic vulcanized rubber masterbatch is blended with a vulcanizer, a first antioxidant, a light stabilizer, a lubricant and a first paraffin oil, and the blended material is added to a screw extruder for a second melting and a second extrusion granulation.

[0022] In an optional embodiment, in the first extrusion granulation step, the temperatures of various zones of the screw extruder are 160~180℃, 180~200℃, 180~200℃, 180~200℃, 180~200℃, 200~220℃, 200~220℃, 190~210℃, 190~210℃, 190~210℃, and 190~210℃, respectively.

[0023] In an optional embodiment, in the second extrusion granulation step, the temperatures in various zones of the screw extruder are 140~160℃, 150~170℃, 160~180℃, 170~190℃, 170~190℃, 180~200℃, 180~200℃, 190~210℃, 190~210℃, 190~210℃, and 190~210℃, respectively.

[0024] In an optional embodiment, the method for preparing the graphene-paraffin oil dispersion includes: dispersing the graphene in a second paraffin oil and ultrasonically dispersing the graphene.

[0025] The present invention has the following beneficial effects:

[0026] The components of the conductive thermoplastic vulcanized rubber provided by the embodiment of the present invention include graphene. The unique two-dimensional structure of graphene enables it to have a large π bond that can penetrate the entire layer of polyatoms, has excellent dielectric loss and conductivity, and the charge can be quickly transferred, so that the composite material can achieve the effects of conductivity, antistatic and electromagnetic shielding; in addition, the mechanical properties of graphene are very excellent and can improve the mechanical properties of the composite material; and the vulcanizer in the component can improve the resilience of the material and improve the mechanical properties of the material, that is, the tensile and tear strength of the material is improved, and the resilience is good. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0028] The thermoplastic vulcanized rubber provided by the related art has poor conductivity, slow heat dissipation, low strength and poor resilience. The present invention provides a conductive thermoplastic vulcanized rubber that can not only be extruded stably and continuously, but also has good conductivity, antistatic, fast heat dissipation, high strength and good resilience.

[0029] The components of the conductive thermoplastic vulcanized rubber of the present invention include, by weight:

[0030] 95~98 parts of thermoplastic vulcanized rubber masterbatch, for example: 95 parts, 96 parts, 97 parts, 98 parts, etc.;

[0031] 0.5~1.2 parts of vulcanizing agent, for example: 0.5 parts, 0.7 parts, 0.9 parts, 1.2 parts, etc.;

[0032] 0.3-0.6 parts of the first antioxidant, for example: 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, etc.;

[0033] Light stabilizer 0.3~0.8 parts, for example: 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.8 parts, etc.;

[0034] Lubricant 0.2~0.5 parts, for example: 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, etc.;

[0035] The first paraffin oil is 0.2 to 0.5 parts, for example: 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, etc.; wherein,

[0036] Thermoplastic vulcanizate masterbatch includes graphene.

[0037] Graphene's unique two-dimensional structure gives it a large π bond that can penetrate the entire layer of multiple atoms, and it has excellent dielectric loss and conductivity. Charges can be transferred quickly, making the composite material conductive, antistatic and electromagnetic shielding. In addition, graphene has excellent mechanical properties and can improve the mechanical properties of the composite material. The vulcanizer in the composition can improve the material's resilience and improve the material's mechanical properties, that is, the material's tensile and tear strength are improved, and its resilience is good.

[0038] In a preferred embodiment, the graphene has a carbon content of 98-99.5wt% (EDS), a sheet diameter of 1-10μm, a thickness of 2~3nm, a moisture content of <2Wt%, a D50 particle size less than or equal to 9um, and a conductivity of 500~600S / cm.

[0039] In some embodiments of the present invention, the thermoplastic vulcanized rubber masterbatch further comprises polypropylene resin, ethylene propylene diene monomer rubber, a second paraffin oil, an inorganic filler, a vulcanizing agent, a second antioxidant, and a masterbatch.

[0040] The present invention adopts long-chain branched EPDM rubber with a relatively large molecular weight, and the length of the rubber entanglement molecular chain is relatively low, which is conducive to the uniform mixing of the rubber phase and the extrusion-grade polypropylene resin. At the same time, multiple organic peroxide vulcanizer phases with different reaction speeds are combined, the vulcanization time is short, and the obtained thermoplastic vulcanized rubber has good heat resistance.

[0041] Optionally, the EPDM rubber has a Mooney viscosity of 85-100, an ethylene content of 40-60%, a third monomer (ENB) content of 4.5-7%, and has controllable long chain branches.

[0042] In a preferred embodiment, the thermoplastic vulcanized rubber masterbatch comprises, by weight, 10 to 20 parts of polypropylene resin (for example, 10 parts, 12 parts, 15 parts, 17 parts, 19 parts, 20 parts, etc.), 25 to 40 parts (for example: 25 parts, 30 parts, 32 parts, 35 parts, 37 parts, 40 parts, etc.), second paraffin oil 20~40 parts (for example: 25 parts, 30 parts, 32 parts, 35 parts, 37 parts, 40 parts, etc.), graphene 2~4 parts (for example: 2 parts, 3 parts, 4 parts, etc.), inorganic filler 5~10 parts (for example: 5 parts, 7 parts, 9 parts, 10 parts, etc.), co-vulcanizing agent 1~3 parts (for example: 1 part, 2 parts, 3 parts, etc.), antioxidant 0.2~0.6 parts (for example: 0.2 parts, 0.4 parts, 0.6 parts, etc.), masterbatch 0.5~2 parts (for example: 0.5 parts, 1 part, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, etc.).

[0043] Optionally, the polypropylene resin is a PP resin having a melt index of about 230° C. and 2.16 kPa and a melt index of 3 g / 10 min.

[0044] Optionally, the inorganic filler may be talcum powder, and the mesh size of the talcum powder is greater than or equal to 3000, and the loss on ignition is 2-3%.

[0045] Optionally, the co-vulcanizing agent is one or more of polybutadiene, butadiene and styrene grafts.

[0046] Optionally, the antioxidant is one or more of the antioxidant 1010 , the antioxidant 168 , the antioxidant 164 , and the antioxidant 264 .

[0047] Optionally, the paraffin oil is a high flash point paraffin oil with a flash point of 230-250°C.

[0048] Optionally, the vulcanizing agent includes one or more of benzoyl peroxide, dicumyl peroxide and di-tert-butyl peroxide.

[0049] Optionally, the light stabilizer is one or more of UV326, UV531, 770 and UV622.

[0050] Optionally, the lubricant is one or more of vinyl bisstearamide, erucamide, zinc stearate, magnesium stearate and polyethylene wax.

[0051] The present invention also provides a method for preparing a conductive thermoplastic vulcanized rubber, comprising:

[0052] preparing a graphene-paraffin oil dispersion;

[0053] The polypropylene resin, EPDM rubber, inorganic filler, vulcanizing agent, second antioxidant and masterbatch are blended, and the blended materials are added into a screw extruder for first melting, and graphene-paraffin oil dispersion is added during the first melting process, and extrusion granulation is performed for the first time to obtain a thermoplastic vulcanized rubber masterbatch;

[0054] The thermoplastic vulcanized rubber masterbatch is blended with a vulcanizer, a first antioxidant, a light stabilizer, a lubricant and a first paraffin oil, and the blended material is added to a screw extruder for a second melting and a second extrusion granulation.

[0055] The preparation method of the conductive thermoplastic vulcanized rubber provided by the present invention prepares graphene into a graphene-paraffin oil dispersion and then adds the dispersion to a screw extruder for extrusion granulation, so that the graphene can be evenly dispersed, thereby ensuring that the conductive thermoplastic vulcanized rubber can be stably and continuously extruded, and has good conductivity, antistatic, fast heat dissipation, high strength and good resilience.

[0056] The method of the present invention first disperses graphene in paraffin oil because the graphene particle size is too small and too thin, and the specific surface area is large, and agglomeration phenomenon is very likely to occur, and it is not easy to be dispersed in the resin. Therefore, graphene is first added to paraffin oil, and the dispersibility of graphene is improved by ultrasonic dispersion, and graphene-paraffin oil dispersion is prepared, which can improve the problem of graphene agglomeration. And to prepare thermoplastic vulcanized rubber elastomer, enough oils must be added in the formulation system as plasticizers, so graphene and paraffin oil are mixed, which can fully improve the dispersibility of graphene on the one hand, and meet the requirements of preparing thermoplastic vulcanized rubber and needing to use oils as plasticizers on the other hand.

[0057] As a dynamic vulcanized rubber, the first granulation of thermoplastic vulcanizate is physical blending. The other materials except the vulcanizing agent are melt blended first, so that each component material is plasticized and dispersed first, and the most important thing is to evenly disperse the rubber component in the polypropylene resin so that the second granulation, vulcanization process, rubber molecular chain crosslinking, and other components are wrapped up. The second granulation is a chemical change after adding the vulcanizing agent. The unstable peroxide groups contained in the organic peroxide decompose to generate free radicals at a certain temperature. The free radicals trigger rubber macromolecules to form rubber free radicals, and crosslinking bonds are formed between macromolecules; linear molecules are connected to each other through this crosslinking method to form a three-dimensional network structure; as the vulcanization process proceeds, this structure is continuously strengthened; in this way, the free activity ability of the chain segment decreases, the plasticity and elongation decrease, the strength, elasticity and hardness increase, and the compression set and swelling degree decrease, so the present invention adopts two granulations.

[0058] It should be noted that the above-mentioned screw extruder may be a twin-screw extruder.

[0059] In some embodiments, the preparation method of the graphene-paraffin oil dispersion includes: dispersing the graphene into the second paraffin oil and dispersing it ultrasonically. The ultrasonic dispersion method can ensure that the graphene is more evenly dispersed in the paraffin oil, so as to improve the uniform dispersion degree of the graphene during subsequent extrusion granulation.

[0060] In a preferred embodiment, in the first extrusion granulation step, the temperatures of each zone of the screw extruder are 160-180°C, 180-200°C, 180-200°C, 180-200°C, 180-200°C, 200-220°C, 200-220°C, 190-210°C, 190-210°C, 190-210°C, and 190-210°C, respectively.

[0061] Furthermore, in the second extrusion granulation step, the temperatures in various zones of the screw extruder are 140-160°C, 150-170°C, 160-180°C, 170-190°C, 170-190°C, 180-200°C, 180-200°C, 190-210°C, 190-210°C, 190-210°C, and 190-210°C, respectively.

[0062] The first granulation belongs to the physical blending of materials. The equipment setting temperature is at the appropriate temperature for the melting of polypropylene resin PP to ensure that PP and EPDM can melt, and the resin can better cover other component materials. Under the shear of the screw, a better blending effect is achieved. If the middle temperature is set higher, the paraffin oil-graphene mixture can be added from the 200-220℃ temperature area of ​​the screw. Since the temperature of the paraffin oil-graphene mixture is relatively low, usually around 70℃, this temperature is not conducive to the melting and plasticization of the material. Therefore, setting the screw temperature at the position where the paraffin oil-graphene mixture is added to a higher temperature is conducive to the melting and plasticization of the material. If the paraffin oil is added from the front end of the screw extruder, the components of the material are not melted and mixed at the beginning. The addition of the paraffin oil liquid will cause the screw to slip, which is not conducive to blending.

[0063] The second granulation involves chemical changes in the raw materials. The masterbatch obtained from the first granulation is vulcanized by adding a vulcanizing agent. The unstable peroxide groups contained in the organic peroxide of the vulcanizing agent decompose to generate free radicals at a certain temperature. The free radicals trigger the rubber macromolecules to form rubber free radicals, and cross-linking bonds are formed between the macromolecules. The most important condition for the vulcanizing agent to take effect is temperature; the temperature setting of the front section of the screw is to ensure that the masterbatch is melted and mixed evenly with the vulcanizing agent, but the vulcanizing agent will not reach the appropriate vulcanization temperature before it is evenly mixed. The vulcanizing agent will not achieve its most effective vulcanization effect until the temperature reaches above 190°C.

[0064] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0065] Example 1

[0066] Preparation:

[0067] (1) Thermoplastic vulcanized rubber masterbatch, components:

[0068] 17 parts of polypropylene resin (PP), 38.8 parts of ethylene propylene diene rubber (EPDM), 2 parts of graphene, 30 parts of paraffin oil, 8 parts of talc, 2 parts of polybutadiene, 0.2 parts of antioxidant (1010), and 2 parts of masterbatch.

[0069] Among them, the carbon content of graphene is 99wt%, the sheet diameter is 10μm, the thickness is 2nm, the water content is <2Wt%, the D50 particle size is 9μm, and the electrical conductivity is 600S / cm.

[0070] The fluid flow rate of polypropylene PP is 1 g / 10 min.

[0071] The Mooney viscosity of EPDM rubber is 85, the ethylene content is 40%, and the content of the third monomer is 4.5%.

[0072] The mesh number of the inorganic filler talc powder is 3000 and the loss on ignition is 2%.

[0073] The flash point of paraffin oil is 230°C.

[0074] (2) Conductive thermoplastic vulcanized rubber, components:

[0075] 97.3 parts of thermoplastic vulcanized rubber masterbatch, 1 part of benzoyl peroxide, 0.4 parts of antioxidant (1010), 0.6 parts of UV326 light stabilizer, 0.5 parts of vinyl bisstearamide, and 0.2 parts of paraffin oil (flash point: 230°C).

[0076] preparation:

[0077] The preparation method of the graphene-paraffin oil dispersion comprises: dispersing graphene in paraffin oil, and ultrasonically dispersing to obtain the graphene-paraffin oil dispersion;

[0078] Polypropylene resin, EPDM rubber, inorganic filler, vulcanizing agent, antioxidant and masterbatch are blended, and the blended materials are added into a screw extruder for first melting, and graphene-paraffin oil dispersion is added during the first melting process, and granulation is performed for the first time to obtain thermoplastic vulcanized rubber masterbatch; wherein the temperatures of various zones of the screw extruder are 160°C, 180°C, 180°C, 180°C, 200°C, 200°C, 190°C, 190°C, 200°C, and 210°C, respectively.

[0079] The thermoplastic vulcanized rubber masterbatch is blended with a vulcanizer, an antioxidant, a light stabilizer, a lubricant and paraffin oil, and the blended material is added to a screw extruder for a second melting and a second extrusion granulation; wherein the temperatures of various zones of the screw extruder are 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 200°C, 200°C, 210°C, 210°C, 210°C.

[0080] Example 2

[0081] Preparation:

[0082] (1) Thermoplastic vulcanized rubber masterbatch, components (the difference between Example 2 and Example 1 is that the amount of graphene used is greater):

[0083] 17 parts of polypropylene resin (PP), 38.8 parts of ethylene propylene diene monomer rubber (EPDM), 4 parts of graphene, 30 parts of paraffin oil, 6 parts of talc, 2 parts of a mixture of diphenylthiourea and butadiene, 0.2 parts of antioxidant (168), and 2 parts of masterbatch.

[0084] Among them, the carbon content of graphene is 98wt%, the sheet diameter is 1μm, the thickness is 3nm, the water content is <2Wt%, the D50 particle size is 8μm, and the electrical conductivity is 500S / cm.

[0085] The fluid flow rate of polypropylene PP is 3 g / 10 min.

[0086] The Mooney viscosity of EPDM rubber is 100, the ethylene content is 60%, and the content of the third monomer is 7%.

[0087] The mesh number of the inorganic filler talc powder is 3000 and the loss on ignition is 3%.

[0088] The flash point of paraffin oil is 250°C.

[0089] (2) Conductive thermoplastic vulcanized rubber, components:

[0090] 97.3 parts of thermoplastic vulcanized rubber masterbatch, 1 part of dicumyl peroxide, 0.4 parts of antioxidant (168), 0.6 parts of UV531 light stabilizer, 0.5 parts of a mixture of erucamide and zinc stearate, and 0.2 parts of paraffin oil (flash point: 250°C).

[0091] preparation:

[0092] The preparation method of the graphene-paraffin oil dispersion comprises: dispersing graphene in paraffin oil, and ultrasonically dispersing to obtain the graphene-paraffin oil dispersion;

[0093] Polypropylene resin, EPDM rubber, inorganic filler, vulcanizing agent, antioxidant and masterbatch are blended, and the blended materials are added into a screw extruder for first melting, and graphene-paraffin oil dispersion is added during the first melting process, and granulation is performed for the first time to obtain thermoplastic vulcanized rubber masterbatch; wherein the temperatures of various zones of the screw extruder are 160°C, 180°C, 180°C, 180°C, 200°C, 200°C, 190°C, 190°C, 200°C, and 210°C, respectively.

[0094] The thermoplastic vulcanized rubber masterbatch is blended with a vulcanizer, an antioxidant, a light stabilizer, a lubricant and paraffin oil, and the blended material is added to a screw extruder for a second melting and a second extrusion granulation; wherein the temperatures of various zones of the screw extruder are 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 200°C, 200°C, 210°C, 210°C, 210°C.

[0095] Example 3

[0096] Preparation:

[0097] (1) Thermoplastic vulcanized rubber masterbatch, components (the difference between Example 3 and Example 1 is that the amount of graphene used is greater):

[0098] Polypropylene resin (PP) 17 parts, ethylene propylene diene monomer rubber (EPDM) 38.8 parts, graphene 3 parts, paraffin oil 30 parts, talc 7 parts, styrene grafted compound 2 parts, antioxidant (168) 0.2 parts, masterbatch 2 parts.

[0099] Among them, the carbon content of graphene is 99.5wt%, the sheet diameter is 5μm, the thickness is 2.5nm, the water content is <2Wt%, the D50 particle size is 9μm, and the conductivity is 550S / cm.

[0100] The fluid flow rate of polypropylene PP is 2 g / 10 min.

[0101] The Mooney viscosity of EPDM rubber is 90, the ethylene content is 50%, and the content of the third monomer is 5%.

[0102] The mesh number of the inorganic filler talc powder is 3000 and the loss on ignition is 2%.

[0103] The flash point of paraffin oil is 240°C.

[0104] (2) Conductive thermoplastic vulcanized rubber, components:

[0105] 97.3 parts of thermoplastic vulcanized rubber masterbatch, 1 part of di-tert-butyl peroxide, 0.4 parts of antioxidant (168), 0.6 parts of UV622 light stabilizer, 0.5 parts of a mixture of magnesium stearate and polyethylene wax, and 0.2 parts of paraffin oil (flash point: 240°C).

[0106] preparation:

[0107] The preparation method of the graphene-paraffin oil dispersion comprises: dispersing graphene in paraffin oil, and ultrasonically dispersing to obtain the graphene-paraffin oil dispersion;

[0108] Polypropylene resin, EPDM rubber, inorganic filler, vulcanizing agent, antioxidant and masterbatch are blended, and the blended materials are added into a screw extruder for first melting, and graphene-paraffin oil dispersion is added during the first melting process, and granulation is performed for the first time to obtain thermoplastic vulcanized rubber masterbatch; wherein the temperatures of various zones of the screw extruder are 160°C, 180°C, 180°C, 180°C, 200°C, 200°C, 190°C, 190°C, 200°C, and 210°C, respectively.

[0109] The thermoplastic vulcanized rubber masterbatch is blended with a vulcanizer, an antioxidant, a light stabilizer, a lubricant and paraffin oil, and the blended material is added to a screw extruder for a second melting and a second extrusion granulation; wherein the temperatures of various zones of the screw extruder are 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 200°C, 200°C, 210°C, 210°C, 210°C.

[0110] Example 4

[0111] The difference between Example 4 and Example 1 is that the components for preparing the thermoplastic vulcanized rubber masterbatch include:

[0112] 10 parts of polypropylene resin (PP), 40 parts of ethylene propylene diene rubber (EPDM), 2 parts of graphene, 34.4 parts of paraffin oil, 10 parts of talc, 1 part of polybutadiene, 0.6 parts of antioxidant (1010), and 2 parts of masterbatch.

[0113] The components for preparing conductive thermoplastic vulcanizate include:

[0114] 96.4 parts of thermoplastic vulcanized rubber masterbatch, 1.2 parts of benzoyl peroxide, 0.6 parts of antioxidant (1010), 0.8 parts of UV326 light stabilizer, 0.5 parts of vinyl bisstearamide, and 0.5 parts of paraffin oil (flash point: 230°C).

[0115] Other parameters refer to Example 1.

[0116] Comparative Example 1

[0117] The difference between Comparative Example 1 and Example 1 is that the amount of graphene in the masterbatch is 0, and the amount of inorganic filler is 10; other process parameters are all referred to Example 1.

[0118] Comparative Example 2

[0119] The difference between Comparative Example 2 and Example 1 is that no EPDM rubber is added to the masterbatch, and the amount of EPDM rubber is supplemented by polypropylene resin; other process parameters are all referred to Example 1.

[0120] Comparative Example 3

[0121] The difference between Comparative Example 3 and Example 1 is that the amount of graphene in the masterbatch is 1 part, the amount of inorganic filler is 9 parts, the amount of EPDM rubber is 10 parts, and the amount of EPDM rubber is supplemented with polypropylene resin; other process parameters are all referred to Example 1.

[0122] Comparative Example 4

[0123] The difference between Comparative Example 4 and Example 1 is that the Mooney viscosity of the EPDM rubber is 30; other process parameters are all referenced to Example 1.

[0124] Comparative Example 5

[0125] The difference between Comparative Example 5 and Example 1 is that the amount of polypropylene PP is 5 parts, and EPDM rubber is used to make up the amount of PP; other process parameters are all referenced to Example 1.

[0126] Comparative Example 6

[0127] The difference between Comparative Example 6 and Example 1 is that the fluid flow rate of polypropylene PP is 20 g / 10 min; other process parameters are all referenced to Example 1.

[0128] Comparative Example 7

[0129] The difference between Comparative Example 7 and Example 1 is that the amount of vulcanizer is 2 parts and the thermoplastic vulcanized rubber masterbatch is 96.3 parts; other process parameters are all referenced to Example 1.

[0130] Comparative Example 8

[0131] The difference between Comparative Example 8 and Example 1 is that the amount of vulcanizer is 0.3 parts, and the thermoplastic vulcanized rubber masterbatch is 98.0 parts; other process parameters are all referred to Example 1.

[0132] Comparative Example 9

[0133] The difference between Comparative Example 9 and Example 1 is that the preparation of the thermoplastic vulcanized rubber masterbatch does not contain antioxidants and paraffin oil. When preparing the thermoplastic vulcanized rubber, the graphene is directly blended with the resin material without ultrasonic dispersion with the paraffin oil. Other process parameters are referred to Example 1.

[0134] Comparative Example 10

[0135] The difference between Comparative Example 10 and Example 1 is that in the first extrusion granulation step, the temperature of each zone of the screw extruder is 170° C.; other process parameters are all referenced to Example 1.

[0136] The materials prepared in various embodiments and comparative examples were tested, and the results are shown in Table 1.

[0137] Table 1

[0138]

[0139] Note: The smaller the material's compression permanent deformation and resistivity, the better; the higher the strength, the better; there is no good or bad judgment for hardness.

[0140] Comparative Example 1 does not add graphene, and the tensile strength and tear strength are reduced, and the resistance is high and the conductive effect is poor.

[0141] Although the tensile strength and tear strength of the comparative example 2 without adding EPDM rubber are high, the elongation at break is low, the Shore hardness is high, the compression permanent deformation is high, and the resilience is poor.

[0142] Comparative Example 3 has less graphene and EPDM rubber than Example 1. Although the tensile strength and tear strength are high, the elongation at break is low, the Shore hardness is high, the compression permanent deformation is high, the resilience is poor, the resistance is high, and the conductive effect is poor.

[0143] The EPDM rubber of Comparative Example 4 has low Mooney viscosity, high compression set and poor resilience.

[0144] In Comparative Example 5, the amount of polypropylene is reduced and the amount of EPDM rubber is increased, the elongation at break is increased, but the tensile strength is reduced, the tear strength is reduced, the compression permanent deformation is high, the resilience is poor, and the Shore hardness is low.

[0145] The fluid flow rate of the polypropylene PP in Comparative Example 6 is 20 g / 10 min, with good fluidity and low viscosity, resulting in high pressure change, high compression permanent deformation and poor resilience.

[0146] In Comparative Example 8, the amount of vulcanizing agent is reduced, the amount of talc is increased, the elongation at break is reduced, the compression permanent deformation is high, and the resilience is poor.

[0147] Comparative Example 9 did not use oil to disperse the graphene first, so the tensile strength and tear strength were low, the resistance was high, and the conductivity was poor.

[0148] In Comparative Example 10, the temperatures of various regions of the screw extruder were not controlled separately, and when the paraffin oil-graphene mixture was added, the temperature was low; the elongation at break was reduced, the compression permanent deformation was high, and the resilience was poor.

[0149] In summary, the conductive thermoplastic vulcanized rubber of the present invention can not only be extruded stably and continuously, but also has good conductivity, antistatic properties, fast heat dissipation, high strength and good resilience.

[0150] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A conductive thermoplastic vulcanized rubber, characterized in that: The components of the conductive thermoplastic vulcanized rubber include, by weight: Thermoplastic vulcanized rubber masterbatch 95-98 parts; Vulcanizing agent 0.5~1.2 parts; 0.3-0.6 parts of the first antioxidant; Light stabilizer 0.3~0.8 parts; Lubricant 0.2~0.5 parts; 0.2-0.5 parts of the first paraffin oil; wherein, The thermoplastic vulcanized rubber masterbatch includes graphene; The thermoplastic vulcanized rubber masterbatch comprises, by weight: 10-20 parts of polypropylene resin, 25-40 parts of EPDM rubber, 20-40 parts of the second paraffin oil, 2-4 parts of the graphene, 5-10 parts of inorganic filler, 1-3 parts of vulcanizing agent, 0.2-0.6 parts of the second antioxidant, and 0.5-2 parts of masterbatch; The graphene has a carbon content of 98-99.5wt%, a sheet diameter of 1-10μm, a thickness of 2-3nm, a moisture content of less than 2Wt%, a D50 particle size of less than or equal to 9μm, and an electrical conductivity of 500-600S / cm; The preparation method of the conductive thermoplastic vulcanized rubber comprises: Dispersing graphene in the second paraffin oil and dispersing by ultrasonic to obtain a graphene-paraffin oil dispersion; The polypropylene resin, EPDM rubber, inorganic filler, vulcanizing agent, second antioxidant and masterbatch are blended, and the blended materials are added into a screw extruder for first melting, and the graphene-paraffin oil dispersion is added during the first melting process, and the thermoplastic vulcanized rubber masterbatch is prepared by extrusion granulation for the first time; The thermoplastic vulcanized rubber masterbatch is blended with a vulcanizer, a first antioxidant, a light stabilizer, a lubricant and a first paraffin oil, and the blended material is added to a screw extruder for a second melting and a second extrusion granulation.

2. The conductive thermoplastic vulcanizate according to claim 1, characterized in that: The Mooney viscosity of the EPDM rubber is 85-100, the ethylene content is 40-60%, and the content of the third monomer is 4.5-7%.

3. The method for preparing a conductive thermoplastic vulcanizate according to claim 2, characterized in that: include: Dispersing graphene in the second paraffin oil and dispersing by ultrasonic to obtain a graphene-paraffin oil dispersion; The polypropylene resin, EPDM rubber, inorganic filler, vulcanizing agent, second antioxidant and masterbatch are blended, and the blended materials are added into a screw extruder for first melting, and the graphene-paraffin oil dispersion is added during the first melting process, and the thermoplastic vulcanized rubber masterbatch is prepared by extrusion granulation for the first time; The thermoplastic vulcanized rubber masterbatch is blended with a vulcanizer, a first antioxidant, a light stabilizer, a lubricant and a first paraffin oil, and the blended material is added to a screw extruder for a second melting and a second extrusion granulation.

4. The method for preparing the conductive thermoplastic vulcanizate according to claim 3, characterized in that: In the first extrusion granulation step, the temperatures of various zones of the screw extruder are 160-180°C, 180-200°C, 180-200°C, 180-200°C, 180-200°C, 200-220°C, 200-220°C, 190-210°C, 190-210°C, 190-210°C, and 190-210°C, respectively.

5. The method for preparing the conductive thermoplastic vulcanizate according to claim 3, characterized in that: In the second extrusion granulation step, the temperatures of various zones of the screw extruder are 140-160°C, 150-170°C, 160-180°C, 170-190°C, 170-190°C, 180-200°C, 180-200°C, 190-210°C, 190-210°C, 190-210°C, and 190-210°C, respectively.

Citation Information

Patent Citations

  • Preparation method of graphene-containing oil-filled solution polymerized butadiene styrene rubber composite material

    CN108129718A

  • Extrusion grade thermoplastic vulcanized rubber and preparation method thereof

    CN115058086A