Submerged arc furnace equipment and method for reducing iron with hydrogen

By using side blower vents to spray a mixed gas of hydrogen and nitrogen in the mine furnace equipment, combined with secondary combustion technology, the problems of high technical difficulty, low output and high cost in the smelting process with hydrogen reduction iron are solved, and high efficiency is achieved , low-carbon iron smelting and waste reuse.

CN115852078BActive Publication Date: 2024-11-22SHERI ENERGY TRADING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211577381.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-22
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

In the prior art, it is difficult to produce pure iron using hydrogen as a reducing agent, with small output and high production costs, and the product cannot be used directly as steelmaking materials.

Method used

Design an ore furnace equipment that reduces iron with hydrogen, uses a mixed gas of hydrogen and nitrogen in the side blower vent. Through the double-layer blower casing structure and secondary combustion technology, the furnace body design is optimized to achieve an efficient iron smelting process. .

Benefits of technology

It significantly improves the output and output efficiency of pig iron, reduces carbon emissions, reduces production costs, and achieves efficient smelting and reuse of tailings, mineral powder and low-grade ore.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852078B_ABST
    Figure CN115852078B_ABST
Patent Text Reader

Abstract

The present invention discloses a submerged arc furnace device for reducing iron with hydrogen and a method for reducing iron with hydrogen in the submerged arc furnace device. The present invention optimizes and transforms the structure of the submerged arc furnace, adds upper and lower rows of side blowing tuyere, and adds hydrogen to the ore melt melted by electric energy by injection. The injection of hydrogen forms a certain flow field in the ore melt, so that hydrogen and iron oxide fully react chemically to generate H2O, thereby realizing an ironmaking process with zero carbon emissions from pig iron. The present invention has low requirements for raw materials, a wide range of raw material sources, high production efficiency, and can achieve intelligent and semi-continuous production. The present invention changes the traditional production process, simplifies the process of hydrogen smelting iron, and has a positive role in reducing carbon emissions and achieving carbon neutrality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal smelting, and in particular to a submerged arc furnace device and method for reducing iron with hydrogen. Background Art

[0002] In the traditional method of producing pig iron, carbon is used as fuel to generate heat energy in a submerged arc furnace, and at the same time as a reducing agent to reduce iron ore to iron. This traditional method has many defects, such as the production of a large amount of carbon monoxide during the production process. As the international requirements for environmental protection continue to increase, especially for carbon emissions, higher requirements are constantly being put forward. Therefore, how to improve the level of technical equipment and optimize the production process to reduce the generation of carbon monoxide has become an urgent problem to be solved in the metallurgical industry at home and abroad.

[0003] At present, there is a method of adding a certain amount of hydrogen during the iron smelting process in a blast furnace to reduce the production of carbon monoxide and reduce carbon emissions; there is also a method of producing pure iron by direct reduction, that is, using hydrogen as a reducing agent to produce pure iron at a certain temperature and pressure. Chinese invention patent CN202011238747.2 discloses a method of utilizing renewable energy electricity, which uses renewable energy electricity to electrolyze water to produce hydrogen and oxygen, and the hydrogen enters a gas-based vertical furnace as a reducing agent to produce sponge iron. However, its equipment is complex, the production is difficult, the output is small, the production cost is high, the raw materials are required to be high, and the reduced iron produced is in powder form and difficult to transport. Steel companies cannot use this powdered reduced iron product directly as a steelmaking raw material, and need to be processed into pressed iron blocks before use. Summary of the invention

[0004] The purpose of the present invention is to solve the problems in the prior art that the production of pure iron using hydrogen as a reducing agent is technically difficult, has a low output, has a high production cost, and the product cannot be directly used as a steelmaking material, and to provide a submerged arc furnace device and method for reducing iron using hydrogen.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: a submerged arc furnace equipment for reducing iron with hydrogen, the submerged arc furnace equipment comprising a furnace shell, a furnace cavity is arranged in the furnace shell, the furnace shell comprises a top, a bottom and a side wall, a slag discharge port and an iron outlet are arranged at the lower end of the side wall of the furnace shell, the iron outlet is arranged close to the bottom of the furnace shell, and the slag discharge port is arranged above the iron outlet; a plurality of side blowing ports are arranged on the side wall of the furnace shell, the plurality of side blowing ports are arranged away from the iron outlet, and a blowing sleeve is arranged in each side blowing port; a plurality of sampling ports are arranged at the upper end of the side wall of the furnace shell, and the sampling ports are arranged above the plurality of side blowing ports; an electric heating rod is arranged at the center of the top of the furnace shell, the electric heating rod penetrates the top of the furnace shell from top to bottom and extends into the furnace cavity, and a plurality of feed ports, hot air ports and smoke exhaust ports are arranged on the top of the furnace shell.

[0006] Preferably, the multiple side air blowing outlets are arranged in two rows, namely an upper row of side air blowing outlets and a lower row of side air blowing outlets. The upper row of side air blowing outlets is arranged in the middle of the side wall of the furnace shell, and the lower row of side air blowing outlets is spaced below the upper row of side air blowing outlets.

[0007] Preferably, the blowing sleeve comprises a central tube and an annular seam tube, the annular seam tube is hollowly sleeved outside the central tube, and an annular air duct is arranged between the central tube and the annular seam tube.

[0008] The present invention also provides a method for reducing iron with hydrogen in the above-mentioned ore-fired furnace equipment, which is characterized by comprising the following steps:

[0009] S1. Add pig iron and slag as bottom materials in the ore-fired furnace, turn on electricity to melt, and form an initial molten pool; add raw materials, and feed nitrogen through the central tube and annular seam tube of the upper and lower rows of side tuyere to form a stable molten pool;

[0010] S2. When the raw materials in the ore-heating furnace are completely melted and the slag temperature is ≧1510°C, the main reduction stage operation is started for 0.9 to 1.5 hours. The central tube gas of the upper and lower side blast ports of the ore-heating furnace is switched to a mixed gas of hydrogen and nitrogen. The annular seam tube of the upper side blast port is still equipped with nitrogen; the annular seam tube of the lower side blast port is switched to a mixture of nitrogen and fine iron ore powder. The content of fine iron ore powder in the mixture is 0.5 to 5 kg / m 3 ; When the hydrogen content above the slag layer of the electric arc furnace is ≧28%, hot air supply begins.

[0011] S3, stop the hot air supply, start the reduction stage operation, the time is 0.65 ~ 0.9 hours, add the direct reduced iron with a pre-reduction degree greater than 63% into the ore furnace, the gas and flow rate in the annular seam pipes of the upper and lower rows of side blast ports are consistent with S2; the central pipes of the upper and lower rows of side blast ports are passed with a mixed gas of hydrogen and nitrogen, the ratio of hydrogen to nitrogen is 1:3, and the flow rate is 83 ~ 92m 3 / min, pressure is 0.6~0.81MPa, when the slag temperature drops to 1150~1200℃, increase the hydrogen ratio in the center tube of the side tuyere, when the slag temperature drops to 1100~1150℃, the center tube is full of hydrogen;

[0012] Preferably, the raw materials in S1 are iron-containing raw materials and slag-making materials that have been dried and pre-reduced, and the iron-containing raw materials that have been dried and pre-reduced include one or more of tailings, ore powder, and low-grade ore.

[0013] Preferably, in S1, the nitrogen flow rate of the central tube is 25-29m 3 / min, the nitrogen flow rate of the annular seam pipe is 11~14m 3 / min.

[0014] Preferably, in S2, the flow rate of the mixed gas in the central tube of the upper row of side blowing ports is 109-125m 3 / min, pressure 0.6~0.82MPa, weight ratio of hydrogen and nitrogen 1:0.2~5, annular pipe nitrogen flow rate 26~32m 3 / min, pressure 0.5~0.59MPa; the flow rate of the mixed gas in the central tube of the lower side blowing outlet is 117~132m 3 / min, pressure 0.6~0.72MPa, weight ratio of hydrogen and nitrogen 1:0.2~5, flow rate of mixture in annular seam pipe 29~37m 3 / min, pressure is 0.5~0.61MPa.

[0015] More preferably, in S2, the hot air flow rate is 15 to 20 m 3 / min, the hot air temperature is 1150~1250℃.

[0016] More preferably, in S3, the amount of direct reduced iron with a pre-reduction degree greater than 63% added is 20-30% of the weight of the melt in the ore-fired furnace.

[0017] More preferably, in S3, a slag-forming agent is added to adjust the pH value of the slag to 1.2-1.4.

[0018] The present invention optimizes the furnace body design of the submerged arc furnace, and adopts the technology of spraying hydrogen from the side tuyere and introducing hot air from the hot tuyere on the furnace shell to achieve a higher secondary combustion rate and secondary combustion heat transfer efficiency. The furnace shell of the submerged arc furnace is provided with upper and lower rows of side blowing tuyere, and each of the side blowing tuyere is provided with a blowing sleeve, which is a double-layer sleeve with a central tube and an annular seam tube. In the side blowing structure design, the side blowing tuyere is arranged in two layers near the slag layer. During the reduction process, the protective gas N 2 The fine-grained iron concentrate is sprayed from the lower side tuyere into the molten slag layer, stirring the slag layer as necessary, and reacting with a large amount of metallic iron in the slag layer to generate FeO. Reducing hydrogen is sprayed from the higher upper side tuyere from the surface of the molten pool to reduce the FeO in the slag to metallic iron. At the same time, the overflowing unreduced hydrogen is secondary burned under the hot air (not less than 1150℃) blown in from the hot tuyere on the top of the furnace to melt the solid raw materials added to the top of the furnace, greatly improving the energy utilization efficiency. The upper part of the molten pool has a strong reaction, and the secondary combustion heat transfer speed is fast. The side injection causes strong stirring of the molten pool and produces a large number of droplets, which provides favorable conditions for forming an ideal heat transfer zone above the molten pool. The metal droplets enter the upper space like the splash formed by the fountain, quickly bringing the heat of the combustion zone into the molten pool, so that the metallic iron and FeO content in the slag form a gradient distribution, and the best reduction effect can be obtained. The rate of metallic iron generation can also be controlled by adjusting the ratio of nitrogen and hydrogen in the injection gas.

[0019] The present invention adopts large slag operation, and the volume ratio of slag to charge is 0.8-1.2. A part of hydrogen in the slag directly reduces the liquid iron oxide therein into iron droplets, and the other part circulates in the slag and partially burns with oxygen in the hot air. Large slag operation can absorb the heat of secondary combustion, prevent the splashing of molten iron, and effectively reduce the iron content in the slag, reduce dust escape, and prevent the re-oxidation of metallic iron.

[0020] The beneficial effects of the present invention are:

[0021] 1) The present invention uses a spraying method to add hydrogen to the ore melt melted by electric energy, and the ore melt is formed into a certain flow field by the spraying of hydrogen, so that the hydrogen and the iron oxides can fully react chemically, thereby realizing efficient smelting of pig iron; the present invention sprays a mixture of nitrogen and fine iron powder while spraying hydrogen in the main reduction stage, so that the stirring effect of the molten pool is enhanced and the reduction rate of high-order iron oxides is accelerated, thereby further improving the output efficiency of pig iron and significantly increasing the output of pig iron;

[0022] 2) The present invention only needs to add two rows of side blowing vents on the furnace shell of the existing submerged arc furnace to complete the transformation of the submerged arc furnace. The structural transformation is simple and uncomplicated, does not change the main structure of the submerged arc furnace, has low transformation cost, and is suitable for wide promotion and application in industry;

[0023] 3) In the present invention, hydrogen is used instead of carbon as a reducing agent. The H2O generated by the combination of hydrogen and oxygen eliminates the generation of carbon monoxide and carbon dioxide in the process of iron production, which completely changes the traditional carbon reduction iron method and effectively reduces carbon emissions in the production process;

[0024] 4) The raw materials used in the present invention are iron-containing raw materials that have been dried and pre-reduced, mainly containing tailings, ore powder and low-grade ore with a particle size greater than 3mm and an iron content less than 40%, and some metallurgical iron-containing waste is added to mix and batch to ensure that the total iron content TFe is ≥45%; the tailings, ore powder and low-grade ore in the iron-containing raw materials are all wastes generated by mining, and the waste is used to achieve efficient smelting of pig iron, achieve the purpose of waste utilization, reduce environmental pollution, and also significantly reduce production costs;

[0025] 5) The main energy source for smelting in the present invention is electricity, and the introduced hydrogen can also be used as an auxiliary fuel to reduce electricity consumption. At the same time, by blowing hot air during the reduction process, a high secondary combustion rate is obtained, which further improves energy utilization and further reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a structural schematic diagram of the ore-fired furnace equipment in the present invention.

[0027] In the figure: 1-furnace shell, 2-iron outlet, 3-slag outlet, 4-blowing sleeve, 401-center tube, 402-annular seam tube, 5-furnace chamber, 6-smoke exhaust port, 7-electric heating rod, 8-upper side air outlet, 9-hot air outlet, 10-feeding port, 11-sampling port, 12-lower side air outlet. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0029] Example 1 A submerged arc furnace apparatus for reducing iron with hydrogen

[0030] A submerged arc furnace device for reducing iron with hydrogen, the submerged arc furnace device comprising a furnace shell 1, a furnace chamber 5 is arranged in the furnace shell 1, the furnace shell comprises a top, a bottom and a side wall, a slag discharge port 3 and an iron outlet 2 are arranged at the lower end of the side wall of the furnace shell 5, the iron outlet is arranged close to the bottom of the furnace shell, and the slag discharge port 3 is arranged above the iron outlet 2; a plurality of side blowing ports are arranged on the side wall of the furnace shell 5, the plurality of side blowing ports are arranged away from the iron outlet, and a blowing sleeve is arranged in each side blowing port; the plurality of side blowing ports are arranged in upper and lower rows of equal number, namely an upper row of side blowing ports 8 and a lower row of side blowing ports 12, the upper row of side blowing ports 8 are arranged in the middle of the side wall of the furnace shell, and the lower row of side blowing ports 12 are arranged below the upper row of side blowing ports 8 at intervals. The blowing sleeve includes a central tube 401 and an annular seam tube 402. The annular seam tube 402 is hollowly sleeved outside the central tube 401. An annular air duct is arranged between the central tube 401 and the annular seam tube 402. Different gases can be introduced into the central tube 401 and the annular seam tube 402 respectively. Two sampling ports 11 are arranged at the upper end of the side wall of the furnace shell 5, and the sampling ports 11 are arranged above the side blowing ports. An electric heating rod 7 is arranged at the center of the top of the furnace shell 1. The electric heating rod 7 passes through the top of the furnace shell 1 and extends into the furnace cavity 5. A feed port 10, a hot air port 9 and a smoke exhaust port 6 are arranged on the top of the furnace shell 1.

[0031] In this embodiment, the feed port 10 is provided with a feed system, the smoke exhaust port 6 is provided with a smoke exhaust system, and the sampling port 11 is provided with a sampling system; the feed system, the smoke exhaust system and the sampling system are all prior art. The feed system can realize automatic loading, automatic weighing and automatic unloading. The sampling system sets sampling ports 11 at different parts of the furnace chamber 5, and uses a small gun-type sampler to regularly collect molten iron and slag samples, continuously analyzes the furnace gas composition to calculate the secondary combustion rate, and adjusts the hot air supply; the molten iron in the slag is obtained by immersing the slag with a sampling cup, and the dust sample in the exhaust gas is taken. The smoke exhaust system uses an external high-temperature fan to extract the smoke out of the ore-fired furnace, passes through the sedimentation chamber to remove coarse particles, smoke, etc., and then passes through the burner to burn out the combustible gas, and then re-enters the furnace chamber 5 through the hot air port 9 for heating the material.

[0032] Example 2 Process for reducing iron with hydrogen in a submerged arc furnace

[0033] The submerged arc furnace equipment is shown in Example 1. In the submerged arc furnace equipment, hydrogen is used to reduce iron. The specific steps are as follows:

[0034] 1. First add pig iron and slag as bottom materials into the furnace chamber of the ore-fired furnace, and then turn on the power to melt to form an initial molten pool. Pig iron and slag are commonly used materials in this technical field. The control target value of the pig iron weight added to the total weight of the raw materials is 22%; the control target value of the slag weight added to the total weight of the raw materials is 15.5%.

[0035] The dried and pre-reduced iron-containing raw materials and slag-making materials are transported to the submerged arc furnace. During the charging and melting process, nitrogen is supplied to the central tube of the side tuyere with a control target value of 25m 3 / min, the target value of nitrogen supply to the annular seam pipe is 11m 3 / min. The dried and pre-reduced iron-containing raw materials include ore powder with a particle size greater than 3mm and an iron content less than 40%, and part of metallurgical iron-containing waste is added to mix and batch so that the total iron content TFe of the iron-containing raw materials is 48%; the slag-making materials include limestone, light-burned dolomite and fluorite, all of which are prepared with reference to the existing technology.

[0036] 2. Main reduction stage operation. When the materials in the furnace are completely melted, the temperature in the furnace is observed through the automatic temperature measurement system of the ore-fired furnace. When the slag temperature reaches 1510°C, the main reduction stage operation begins.

[0037] According to the online composition analysis system, the composition of slag and molten iron is determined, and the theoretical hydrogen consumption is preliminarily calculated. The calculation equation of theoretical hydrogen consumption is shown in Table 1. The production of 1 ton of molten iron requires about 2.08 tons of dried and pre-reduced iron-containing raw materials. Correspondingly, the production of 1 ton of molten iron consumes 900m3 of hydrogen. 3 About (hydrogen utilization rate 67%). Start gas distribution operation. Start switching the central tube gas of the upper side blowing port to hydrogen plus nitrogen, and the flow control target value is 125m 3 / min, pressure 0.6MPa, annular pipe is still equipped with nitrogen, flow control target value is 32m 3 / min, pressure 0.5MPa; the gas in the center tube of the lower side blowing outlet is hydrogen plus nitrogen, and the flow control target value is 128m 3 / min, pressure 0.6MPa, annular pipe is nitrogen plus fine iron ore powder (purchased), flow control target value is 29m 3 / min nitrogen, the target value of the content of fine iron ore in the mixture is 1.5kg / m 3 , pressure 0.5MPa. The specific ratio of hydrogen to nitrogen in the central tube of the upper and lower rows of side blowing tuyere is gradually increased according to the slagging situation, as shown in Table 2.

[0038] Table 1 Reaction equation for theoretical calculation of hydrogen consumption

[0039] Reaction equation Hydrogen consumption / Kg <![CDATA[Fe2O3+3H2==2Fe+3H2O]]> 1000*55%*95% / 55.85*2*1.5=28 <![CDATA[Fe2O3+H2==2FeO+H2O]]> 1000*55%*5% / 55.85*2*0.5=0.49

[0040] When calculating the theoretical consumption of hydrogen, it is assumed that Fe exists in the form of Fe2O3 and the reduction of other oxides is not considered, of which 95% of Fe2O3 is reduced to Fe and 5% is reduced to FeO. 100% of the pure hydrogen introduced is used to reduce the oxides. Taking 1 ton of iron ore as an example, the specific hydrogen consumption is shown in Table 1.

[0041] Table 2 Specific hydrogen and nitrogen ratios of the central tubes of the upper and lower rows of side blowing outlets

[0042]

[0043]

[0044] According to the composition of furnace gas on the upper surface of slag displayed by the online analyzer, the H2 content in the furnace gas reaches 30%. The hot air pipe is opened and the target value of hot air flow is controlled to 15m 3 / min, the target hot air temperature is 1150℃, forming secondary combustion and accelerating reduction. When the theoretical hydrogen consumption is initially reached, the flow rate of the tuyere center pipe and the annular seam pipe is reduced, and the slag temperature in the furnace is displayed according to the automatic temperature measurement system. The power distribution operation is carried out according to the smelting temperature requirements, and the target slag temperature in the furnace is controlled to be 1560℃. The main reduction stage lasts for 1.5 hours.

[0045] 3. Final reduction operation. Stop the hot air supply from the hot air port. The feed system adds direct reduced iron (prepared by the existing method) with a pre-reduction target value of 63% from the feed port, and adds slag-making agent to adjust the basicity of the slag to a target value of 1.28.

[0046] The gas flow and gas type in the annular seam pipes of the upper and lower rows of side blowing outlets remain unchanged. Hydrogen and nitrogen are passed through the central pipe. The control ratio target value is 1:3, and the flow control target value is 83m 3 / min, pressure 0.6MPa. The slag temperature drops to 1200℃, and the hydrogen ratio in the central tube is increased until it is all hydrogen.

[0047] Combining the molten iron composition obtained by the online composition analysis system with the manual sampling results, the iron content and other element contents meet the requirements for discharge from the furnace, and the deoxidation operation can be completed. The final reduction stage lasts 0.9 hours.

[0048] 4. Iron tapping operation. Qualified molten iron flows out from the iron tapping hole and is cast into iron blocks, and slag flows out from the slag tapping hole. The recovery rate of metallic iron in this embodiment is 88%.

[0049] Example 3

[0050] The submerged arc furnace equipment is shown in Example 1. In the submerged arc furnace equipment, hydrogen is used to reduce iron. The specific steps are as follows:

[0051] 1. First add pig iron and slag as bottom materials into the furnace chamber of the ore-fired furnace, and then turn on the power to melt to form an initial molten pool. Pig iron and slag are commonly used materials in this technical field. The control target value of the pig iron weight added to the total weight of the raw materials is 25%; the control target value of the slag weight added to the total weight of the raw materials is 17%.

[0052] The dried and pre-reduced iron-containing raw materials and slag-making materials are transported to the submerged arc furnace. During the charging and melting process, nitrogen is supplied to the central tube of the side tuyere with a control target value of 27m 3 / min, the target value of nitrogen supply to the annular seam pipe is 14m 3 / min. The dried and pre-reduced iron-containing raw materials include tailings, ore powder and low-grade ores with a particle size greater than 3mm and an iron content less than 40%, and part of metallurgical iron-containing waste is added to mix and batch so that the total iron content TFe of the iron-containing raw materials is 52%; the slag-making materials include limestone, light-burned dolomite and fluorite, all of which are prepared with reference to the existing technology.

[0053] 2. Main reduction stage operation. When the materials in the furnace are completely melted, the temperature in the furnace is observed through the automatic temperature measurement system of the ore-fired furnace. When the slag temperature reaches 1520°C, the main reduction stage operation begins.

[0054] The slag and molten iron components are determined by the online component analysis system, and the theoretical hydrogen consumption is preliminarily calculated. The calculation equation of the theoretical hydrogen consumption is shown in Table 1 in Example 2. The production of 1 ton of molten iron requires about 1.92 tons of dried and pre-reduced iron-containing raw materials. Correspondingly, the production of 1 ton of molten iron consumes 833 m 3 About (hydrogen utilization rate 72%). Start gas distribution operation. Start switching the central tube gas of the upper side blowing port to hydrogen plus nitrogen, and the flow control target value is 118m 3 / min, pressure 0.75MPa, annular pipe is still equipped with nitrogen, flow control target value is 29m 3 / min, pressure 0.55MPa; the gas in the center tube of the lower side blowing outlet is hydrogen plus nitrogen, and the flow control target value is 132m 3 / min, pressure 0.65MPa, annular pipe is nitrogen plus fine iron ore powder (purchased), flow control target value is 33m 3 / min, the target value of the fine iron ore content in the mixture is 2.4kg / m 3 The specific ratio of hydrogen to nitrogen in the central tube of the upper and lower rows of side blowing tuyere is gradually increased according to the slagging situation, as shown in Table 2 in Example 2.

[0055] According to the furnace gas composition on the upper surface of the slag displayed by the online analyzer, when the H2 in the furnace gas reaches 32%, the hot air pipe is opened and the hot air flow rate is controlled at 17m 3 / min, control the hot air temperature target value to 1210℃, form secondary combustion and accelerate reduction. When the theoretical hydrogen consumption is initially reached, reduce the flow of the tuyere main pipe and annular seam, and according to the slag temperature in the furnace displayed by the automatic temperature measurement system, the power distribution operation needs to be carried out according to the smelting temperature, and control the slag temperature target value in the furnace to 1530℃. The main reduction stage lasts for 1.1 hours.

[0056] 3. Final reduction operation. Stop the hot air supply from the hot air port. The feed system adds pre-reduction degree control target value of 70% direct reduced iron (prepared by existing method) from the feed port, and adds slag-making agent to adjust the basicity of the slag to control target value of 1.32.

[0057] The gas flow and gas type in the annular seam pipes of the upper and lower rows of side blowing outlets remain unchanged. Hydrogen and nitrogen are passed through the central pipe. The control ratio target value is 1:3.2, and the flow target control value is 89m 3 / min, pressure 0.75MPa. The slag temperature drops to 1150℃, and the hydrogen ratio in the central tube is increased until it is all hydrogen.

[0058] Combining the molten iron composition obtained by the online composition analysis system with the manual sampling results, the iron content and other element contents meet the requirements for discharge from the furnace, and the deoxidation operation can be completed. The final reduction stage lasts 0.78 hours.

[0059] 4. Iron tapping operation. Qualified molten iron flows out from the iron tapping hole and is cast into iron blocks, and slag flows out from the slag tapping hole. The recovery rate of metallic iron in this embodiment is 92%.

[0060] Example 4

[0061] The submerged arc furnace equipment is shown in Example 1. In the submerged arc furnace equipment, hydrogen is used to reduce iron. The specific steps are as follows:

[0062] 1. First add pig iron and slag as bottom materials into the furnace chamber of the ore-fired furnace, and then turn on the power to melt to form an initial molten pool. Pig iron and slag are commonly used materials in this technical field. The target control value of the pig iron weight added to the total weight of the raw materials is 28%; the target control value of the slag weight added to the total weight of the raw materials is 18.5%.

[0063] The dried and pre-reduced iron-containing raw materials and slag-making materials are transported to the submerged arc furnace. During the charging and melting process, nitrogen is supplied to the central tube of the side tuyere. The target control value is 29m 3 / min, the target control value of nitrogen supply to the annular seam pipe is 13m 3 / min. The dried and pre-reduced iron-containing raw materials include tailings, ore powder and low-grade ores with a particle size greater than 3mm and an iron content less than 40%, and part of metallurgical iron-containing waste is added to mix and batch so that the total iron content TFe of the iron-containing raw materials is 65%; the slag-making materials include limestone, light-burned dolomite and fluorite, all of which are prepared with reference to the existing technology.

[0064] 2. Main reduction stage operation: When the materials in the furnace are completely melted, the temperature in the furnace is observed through the automatic temperature measurement system of the ore-fired furnace. When the slag temperature reaches 1550°C, the main reduction stage operation begins.

[0065] The slag and molten iron components are determined by the online component analysis system, and the theoretical hydrogen consumption is preliminarily calculated. The calculation equation of the theoretical hydrogen consumption is shown in Table 1 in Example 2. The production of 1 ton of molten iron requires about 1.54 tons of dried and pre-reduced iron-containing raw materials. Correspondingly, the production of 1 ton of molten iron consumes 750 m 3 About (hydrogen utilization rate 80%). Start gas distribution operation. Start switching the central tube gas of the upper side blowing port to hydrogen plus nitrogen, and the flow control target value is 109m 3 / min, pressure 0.82MPa, annular pipe is still equipped with nitrogen, flow control target value is 26m 3 / min, pressure 0.59MPa; the gas in the center tube of the lower side blowing port is hydrogen plus nitrogen, and the flow control target value is 117m 3 / min, pressure 0.72MPa, annular pipe is nitrogen plus fine iron ore powder (purchased), flow control target value is 37m 3 / min, pressure 0.61MPa. The specific ratio of hydrogen to nitrogen in the central tube of the upper and lower rows of side blowing tuyere is gradually increased according to the slagging situation, as shown in Table 2 in Example 2.

[0066] According to the furnace gas composition on the upper surface of the slag displayed by the online analyzer, when the H2 in the furnace gas reaches 28%, the hot air pipe is opened and the hot air flow rate is controlled to a target value of 20m 3 / min, control the hot air temperature target value to 1250℃, form secondary combustion and accelerate reduction. When the theoretical hydrogen consumption is initially reached, the flow rate of the tuyere main pipe and the annular seam is reduced, and the slag temperature in the furnace is displayed according to the automatic temperature measurement system. The power distribution operation is carried out according to the smelting temperature requirements, and the target value of the slag temperature in the furnace is controlled to be 1518℃. The main reduction stage lasts for 0.9 hours.

[0067] 3. Final reduction operation. Stop the hot air supply from the hot air port. The feed system adds pre-reduction degree from the feed port to control the target value of 75% direct reduced iron (prepared by the existing method), and adds slag-making agent to adjust the pH value of the slag to control the target value of 1.38.

[0068] The gas flow and gas type in the annular seam pipes of the upper and lower rows of side blowing outlets remain unchanged. Hydrogen and nitrogen are passed through the central pipe. The control ratio target value is 1:2.9, and the flow rate is controlled at 92m 3 / min, pressure 0.81MPa. The slag temperature drops to 1100℃, and the hydrogen ratio in the central tube is increased until it is all hydrogen.

[0069] Combining the molten iron composition obtained by the online composition analysis system with the manual sampling results, the iron content and other element contents meet the requirements for discharge from the furnace, and the deoxidation operation can be completed. The final reduction stage lasts for 0.65 hours.

[0070] 4. Iron tapping operation. Qualified molten iron flows out from the iron tapping hole and is cast into iron blocks, and slag flows out from the slag tapping hole. The recovery rate of metallic iron in this embodiment is 93.5%.

[0071] In summary, the present invention performs a simple structural transformation on the existing submerged arc furnace, adds upper and lower rows of side blowing tuyere (Example 1), adds hydrogen into the ore powder melt melted by electric energy by a blowing method, and sprays a mixture of nitrogen and fine iron concentrate at the same time, so that hydrogen and iron oxide can fully react chemically, and the output efficiency of pig iron in tailings, ore powder and low-grade ore raw materials is significantly improved. The recovery rate of metallic iron in iron-containing raw materials with a total iron content of 48%≦TFe≦65% reaches more than 88% (data of Examples 2-4), realizing efficient smelting of pig iron and recycling of ore waste (tailings, ore powder and low-grade ore with an iron content of less than 40%), and reducing resource waste.

[0072] The specification and drawings of the present invention are considered to be illustrative rather than restrictive. On the basis of the present invention, those skilled in the art can make some substitutions and modifications to some of the technical features according to the disclosed technical content without creative labor, all of which are within the protection scope of the present invention.

Claims

1. A method for reducing iron with hydrogen in a submerged arc furnace. The following steps are involved: S1. Add pig iron and slag as bottom materials into the ore-fired furnace equipment, and melt them by electricity to form an initial molten pool; Add raw materials and feed nitrogen through the central tube and annular seam tube of the upper and lower rows of side tuyere to form a stable molten pool; S2. When the raw materials in the ore-heating furnace are completely melted and the slag temperature is ≥1510°C, the main reduction stage operation is started for 0.9 to 1.5 hours. The central tube gas of the upper and lower side blast ports of the ore-heating furnace is switched to a mixed gas of hydrogen and nitrogen. The annular seam pipe of the upper side blast port is still equipped with nitrogen. The annular seam pipe of the lower side blast port is switched to a mixture of nitrogen and fine iron ore powder. The content of fine iron ore powder in the mixture is 0.5 to 5 kg / m 3 ; When the hydrogen content above the slag layer of the ore-fired furnace is ≥28%, hot air starts to be supplied; S3, stop the hot air supply, start the reduction stage operation, the time is 0.65 ~ 0.9 hours, add the direct reduced iron with a pre-reduction degree greater than 63% into the ore furnace, the gas and flow rate in the annular seam pipes of the upper and lower rows of side blast ports are consistent with S2; the central pipes of the upper and lower rows of side blast ports are passed with a mixture of hydrogen and nitrogen, the ratio of hydrogen to nitrogen is 1:3, and the flow rate is 83 ~ 92m 3 / min, pressure is 0.6~0.81 MPa, when the slag temperature drops to 1150~1200℃, increase the hydrogen ratio in the central tube of the side blowing tuyere, when the slag temperature drops to 1100~1150℃, the central tube is full of hydrogen; The ore-heating furnace equipment comprises a furnace shell, a furnace cavity is arranged in the furnace shell, the furnace shell comprises a top, a bottom and a side wall, a slag discharge port and an iron outlet are arranged at the lower end of the side wall of the furnace shell, the iron outlet is arranged close to the bottom of the furnace shell, and the slag discharge port is arranged above the iron outlet; a plurality of side blowing ports are arranged on the side wall of the furnace shell, the plurality of side blowing ports are arranged away from the iron outlet, and a blowing sleeve is arranged in each side blowing port; a plurality of sampling ports are arranged at the upper end of the side wall of the furnace shell, and the sampling ports are arranged above the plurality of side blowing ports; an electric heating rod is arranged at the center of the top of the furnace shell, the electric heating rod penetrates the top of the furnace shell from top to bottom and extends into the furnace cavity, and a plurality of feed ports, hot air ports and smoke exhaust ports are arranged on the top of the furnace shell.

2. The method according to claim 1, It is characterized in that The multiple side blowing air outlets are arranged in two rows, upper and lower, which are respectively the upper row of side blowing air outlets and the lower row of side blowing air outlets. The upper row of side blowing air outlets is arranged in the middle of the side wall of the furnace shell, and the lower row of side blowing air outlets is arranged below the upper row of side blowing air outlets.

3. The method according to claim 1, It is characterized in that The blowing sleeve comprises a central tube and an annular seam tube, wherein the annular seam tube is hollowly sleeved outside the central tube, and an annular air duct is arranged between the central tube and the annular seam tube.

4. The method according to claim 1, It is characterized in that The raw materials in S1 are iron-containing raw materials and slag-making materials that have been dried and pre-reduced. The iron-containing raw materials that have been dried and pre-reduced include one or more of tailings, ore powder, and low-grade ore.

5. The method according to claim 1, It is characterized in that In S1, the nitrogen flow rate of the central tube is 25-29m 3 / min, the nitrogen flow rate of the annular seam pipe is 11~14m 3 / min.

6. The method according to claim 1, It is characterized in that In S2, the flow rate of the mixed gas in the central tube of the upper side blowing port is 109-125m 3 / min, pressure 0.6~0.82 MPa, weight ratio of hydrogen to nitrogen 1:0.2~5, annular pipe nitrogen flow rate 26~32m 3 / min, pressure 0.5~0.59MPa; the flow rate of the mixed gas in the central tube of the lower side blowing outlet is 117~132m 3 / min, pressure 0.6~0.72 MPa, weight ratio of hydrogen and nitrogen 1:0.2~5, flow rate of mixture in annular seam pipe 29~37m 3 / min, pressure is 0.5~0.61MPa.

7. The method according to claim 1, It is characterized in that In S2, the hot air flow rate is 15-20m 3 / min, the hot air temperature is 1150~1250℃.

8. The method according to claim 1, It is characterized in that In S3, the amount of direct reduced iron with a pre-reduction degree greater than 63% added is 20-30% of the weight of the melt in the ore-fired furnace.

9. The method according to claim 1, It is characterized in that In S3, a slag-forming agent is added to adjust the pH value of the slag to 1.2-1.4.