A method for effectively avoiding the formation of residual tin droplets on the surface of niobium-tin thin films by physical adsorption

By using cold traps and high-purity ceramic sheets to absorb tin vapor during the coating process, the problem of residual tin droplets on the film surface in the tin vapor diffusion method is solved, the performance of the radio frequency superconducting cavity is improved and the process conditions are simplified.

CN115852302BActive Publication Date: 2024-10-18INST OF MODERN PHYSICS CHINESE ACADEMY OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211590083.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-10-18
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

When the existing tin vapor diffusion method is used to prepare Nb3Sn thin films, it is easy to cause nanoscale tin droplets to remain on the surface of the film, which limits the performance of the radio frequency superconducting cavity. The process conditions are complex and it is difficult to effectively suppress the generation of tin droplets.

Method used

By creating a temperature difference during the coating process, a cold trap is formed to absorb residual tin vapor, and high-purity ceramic sheets are suspended in the coating chamber to absorb tin vapor to prevent tin droplets from forming on the surface of the film. Specific steps include turning off the tin source heating power after high-temperature growth to form a low-temperature cold trap, or hanging a high-purity ceramic sheet at the tin vapor outlet to absorb excess tin vapor.

Benefits of technology

It effectively avoids the generation of tin droplets on the surface of the Nb3Sn film, improves the performance of the radio frequency superconducting cavity, reduces the complexity of the tin vapor diffusion process, and appropriately relaxes the precise control of coating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003993775160000011
    Figure HDA0003993775160000011
  • Figure HDA0003993775160000012
    Figure HDA0003993775160000012
  • Figure HDA0003993775160000021
    Figure HDA0003993775160000021
Patent Text Reader

Abstract

The present invention discloses a method for effectively avoiding the generation of residual tin droplets on the surface of a niobium tin film by physical adsorption. The present invention adopts a physical adsorption method to avoid the generation of tin droplets during the coating process, including the following 1) and / or 2): 1) after the high-temperature growth stage during the coating process, the tin source heating power supply at the lower position of the coating cavity is turned off, or the furnace heating belt power supply at the upper position of the coating cavity is turned off to form a low-temperature zone cold trap at the tin vapor inlet and outlet of the coating cavity, and the tin vapor inside the coating cavity is adsorbed by a low-temperature cold trap; 2) during the coating process, a ceramic sheet is arranged at the tin vapor outlet of the coating cavity to adsorb the diffused tin vapor. The physical adsorption method of the present invention can effectively avoid the appearance of tin droplets on the surface of the Nb3Sn film during the coating process, thereby avoiding its influence on the radio frequency superconducting performance of the Nb3Sn film superconducting cavity; the method can appropriately relax the precise control of the coating conditions, thereby greatly reducing the complexity of the tin vapor diffusion process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for effectively avoiding the generation of residual tin droplets on the surface of a niobium-tin film through physical adsorption, and belongs to the technical field of superconductivity. Background Art

[0002] Compared with traditional pure niobium superconducting cavities, Nb3Sn thin film superconducting cavities can operate at higher temperatures and acceleration gradients, thereby significantly reducing the construction and operation costs of superconducting accelerators. It is the core key technology of the next generation of superconducting accelerators. Among the many methods for preparing Nb3Sn thin film superconducting cavities, the tin vapor diffusion method is the method with the best performance and the most application prospects so far. At present, the existing tin vapor diffusion method for Nb3Sn thin film processes will cause some nano-scale tin droplets to remain on the surface of the film. Compared with Nb3Sn (Tc ~ 18K), the superconducting transition temperature of Sn is only 3.7K. The tin droplets on the surface of Nb3Sn will limit the performance of the radio frequency superconducting cavity. Therefore, developing a method to effectively avoid the generation of residual tin droplets on the surface of niobium tin (Nb3Sn) thin films through physical adsorption is of great significance for the application of Nb3Sn thin films in high-performance radio frequency superconductors. Summary of the invention

[0003] The purpose of the present invention is to provide a method for effectively avoiding the generation of residual tin droplets on the surface of a niobium tin (Nb3Sn) film by physical adsorption. The method of the present invention forms a cold trap to adsorb residual tin vapor by creating a temperature difference, suspends high-purity ceramics in a coating chamber to adsorb residual tin vapor and successfully avoids the generation of residual tin droplets on the surface of a growing Nb3Sn film.

[0004] In order to achieve the above object, the present invention avoids the generation of residual tin droplets on the surface of niobium tin (Nb3Sn) film by physical adsorption in the tin vapor diffusion method;

[0005] By physical adsorption, the adsorption of residual tin vapor inside the coating chamber is increased, thereby inhibiting the residual tin vapor from generating tin droplets on the film surface;

[0006] Among them, the tin vapor diffusion method is a conventional method in this field, and can be carried out according to the steps recorded in the following document: Sam Posen, Understanding and overcoming limitation mechanisms in Nb3Snsuperconducting RF cavities, PhD thesis of Cornell University, USA, 2015.

[0007] Specifically, the substrate niobium used in the present invention is pure metal niobium with an RRR value (residual resistivity ratio, characterizing the purity of the material) ≥ 40;

[0008] Specifically, the physical adsorption method disclosed in the present invention comprises the following steps (1) and / or (2):

[0009] (1) After the high temperature growth in the coating process is completed, the tin source heating power supply at the lower position of the coating chamber is turned off, or the furnace heating belt power supply at the upper position of the coating chamber is turned off,

[0010] A low-temperature cold trap is formed at the inlet and outlet of the tin vapor of the coating chamber to form a low-temperature cold trap to absorb the tin vapor inside the coating chamber;

[0011] (2) During the coating process, a high-purity ceramic sheet is arranged at the tin vapor outlet of the coating chamber, and the good adsorption and high temperature resistance of the ceramic are utilized to adsorb the excess tin vapor diffused during the coating growth stage.

[0012] The niobium-tin thin film obtained by the method of the present invention also belongs to the protection scope of the present invention.

[0013] The tin vapor diffusion method is currently the best method for preparing niobium-based Nb3Sn thin film superconducting cavities. The existing tin vapor diffusion process is very likely to leave some nano-scale tin droplets on the surface of the Nb3Sn film, which in turn affects the performance of the RF superconducting cavity. In addition, the conditions for growing high-quality Nb3Sn thin films by the tin vapor diffusion method are complex, and it is difficult to suppress the generation of tin droplets by optimizing the coating process.

[0014] The physical adsorption method provided by the present invention can effectively prevent the appearance of tin droplets on the surface of the Nb3Sn thin film during the coating process, thereby preventing it from affecting the radio frequency superconducting performance of the Nb3Sn thin film superconducting cavity. At the same time, the method can appropriately relax the precise control of the coating conditions (including the amount of tin, the amount of the nucleating agent SnCl2, etc.), thereby greatly reducing the complexity of the tin vapor diffusion process. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a SEM photograph of the surface of the Nb3Sn film prepared in Comparative Example 1 of the present invention.

[0016] Figure 2 This is a SEM photograph of the surface of the Nb3Sn film prepared in Example 1 of the present invention.

[0017] Figure 3 This is a SEM photograph of the surface of the Nb3Sn film prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0018] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0019] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0020] The tin vapor diffusion method used in the following embodiments is carried out according to the steps described in the following documents:

[0021] Sam Posen, Understanding and overcoming limitation mechanisms in Nb3Snsuperconducting RF cavities, PhD dissertation, Cornell University, 2015.

[0022] Comparative Example 1: Preparation of Nb3Sn thin film (original sample)

[0023] The size of the niobium substrate is 4mm×4mm×1.5mm, and the Nb3Sn thin film coating experiment is carried out simultaneously with the pure niobium superconducting cavity by tin vapor diffusion method.

[0024] Among them, the conditions of the tin vapor diffusion method are as follows:

[0025] During the high-temperature growth stage, the temperature of the superconducting cavity is 1100°C and the temperature of the tin source is 1200°C, which are maintained for 3 hours; then the temperature of the tin source is reduced to 1100°C and the temperature of the superconducting cavity is maintained at 1100°C. This stage is the insulation stage and is maintained for 6 hours.

[0026] The Nb3Sn film was degreased, ultrasonically cleaned and dried in turn. The specific method is as follows: the sample was placed in an ultrasonic cleaning solution for 40 minutes at a water temperature of 55°C, wherein the ultrasonic cleaning solution used was 10 ml of Micro-90 cleaning agent added to every 500 ml of deionized water, and after the ultrasonic cleaning was completed, it was rinsed with ultrapure water for 3 times and dried in the air. This step is to remove possible contamination on the surface of Nb3Sn so as not to affect the observation of its surface morphology.

[0027] Example 1. Preparation of Nb3Sn thin film (sample after physical adsorption)

[0028] The niobium substrate has a size of 4mm×4mm×1.5mm, and a tin vapor diffusion method is used to deposit Nb3Sn thin film simultaneously with a pure niobium superconducting cavity. The conditions of the tin vapor diffusion method are the same as those of comparative example 1, and the following treatments are performed during the film deposition process:

[0029] After the high-temperature growth stage of the film is over, the tin source heating power supply is stopped to form a low-temperature cold trap to adsorb the tin vapor that has not completely diffused into the cavity from the tin source area, and the upper heating belt of the cavity heating is turned off, and only the lower heating belt is turned on to form a cold trap with a temperature difference of 27°C between the upper and lower parts of the cavity heating zone. The lower heating belt keeps the cavity temperature at 1100°C at all times, allowing the residual tin vapor that has not completely reacted in the cavity to continue to diffuse to the cold trap area and be adsorbed.

[0030] The Nb3Sn film was subjected to surface degreasing, ultrasonic cleaning and air-drying in sequence, and the specific steps were the same as those in Comparative Example 1.

[0031] Example 2: Preparation of Nb3Sn thin film (sample after physical adsorption)

[0032] The niobium substrate has a size of 4mm×4mm×1.5mm, and a tin vapor diffusion method is used to deposit Nb3Sn thin film simultaneously with a pure niobium superconducting cavity. The vapor diffusion method is the same as in comparative example 1, and the following treatments are performed during the film deposition process:

[0033] Two 99 high-purity ceramic bricks are hung at the tin vapor outlet on the upper part of the coating chamber to absorb residual tin vapor.

[0034] The Nb3Sn film was subjected to surface degreasing, ultrasonic cleaning and air-drying in sequence, and the specific steps were the same as those in Comparative Example 1.

[0035] X-ray photoelectron spectroscopy (XPS) was used to analyze the elemental composition and content of the film surface. The surface Nb / Sn before etching was significantly smaller than that after etching for 50 seconds, which verified the results under the scanning electron microscope that tin spots existed on the surface of the Nb3Sn film.

[0036] The morphological characteristics of the cleaned original Nb3Sn surface (Comparative Example 1) and the Nb3Sn surface after physical adsorption (Examples 1 and 2) were observed by scanning electron microscopy (SEM). Figure 1 , Figure 2 and Figure 3 shown.

[0037] Figure 1 The white spots on the middle surface are the nano-sized tin droplets remaining on the surface of the Nb3Sn film produced by the tin vapor diffusion method; Figure 2 It shows that the removal effect of tin droplets on the surface of Nb3Sn film is obvious after increasing the physical adsorption of tin vapor by making a cold trap in the low temperature zone; Figure 3 It is shown that the tin droplets on the surface of the Nb3Sn film are significantly removed by suspending high-purity ceramic bricks with good thermal stability and strong adsorption to increase the physical adsorption of tin vapor.

Claims

1. A method for preparing a niobium-tin thin film, comprising the steps of preparing the niobium-tin thin film from a niobium substrate by a tin vapor diffusion method; characterized in that: Physical adsorption method is used to avoid the generation of tin droplets during the coating process; The physical adsorption method comprises the following steps 1) or 2): 1) After the high-temperature growth stage in the coating process is over, the tin source heating power supply at the lower position of the coating chamber is turned off, or the furnace heating belt power supply at the upper position of the coating chamber is turned off to form a low-temperature zone cold trap at the tin vapor inlet and outlet of the coating chamber, so as to form a low-temperature cold trap adsorption for the tin vapor inside the coating chamber; 2) During the coating process, a ceramic sheet is arranged at the tin vapor outlet of the coating chamber to absorb the diffused tin vapor.

2. The preparation method according to claim 1, characterized in that: The RRR value of the niobium substrate is ≥40.

Citation Information

Patent Citations

  • Method for effectively treating tin drops on surface of Ni3Sn thin film

    CN114990552A

  • Hot evaporation plant of liquid drop splash baffle is prevented in area

    CN207877846U

  • Vapor deposition apparatus

    JP2006249558A

  • Method for the manufacture of a superconductive nb" 3"sn layer on a niobium surface for high frequency applications

    US4105512A