A tungsten carbide-tungsten sulfide composite catalytic material and its preparation method and application
By one-step synthesis of tungsten carbide-tungsten sulfide thin films on tungsten foil, a vertical scale structure is formed, which solves the problem of tungsten carbide sintering into agglomerates at high temperatures, improves catalytic activity and conductivity, and achieves efficient electrochemical water splitting. hydrogen.
Patent Information
- Application Number
- CN202210260511.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-27
- Filing Date
- 2022-03-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-16
AI Technical Summary
It is difficult to synthesize tungsten carbide nanostructures with high specific surface areas through simple preparation methods in the existing technology, causing them to sinter into blocks at high temperatures, reducing the effective surface area and catalytic activity.
Tungsten foil is used as the substrate and tungsten source, and a tungsten carbide-tungsten sulfide film is synthesized in one step through chemical vapor deposition to form a vertical scale structure, increase the specific surface area and increase the active sites of the catalyst.
The conductivity and number of active sites of the catalyst are improved, and the efficiency and stability of electrochemical water splitting to produce hydrogen are enhanced. The preparation method is simple to operate, low in cost, and suitable for mass production.
Smart Images

Figure CN115852387B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a tungsten carbide-tungsten sulfide composite catalytic material and a preparation method and application thereof, belonging to the technical field of electrochemical water decomposition to produce hydrogen. Background Art
[0002] The use of hydrogen energy can reduce the combustion of fossil fuels, thereby avoiding environmental pollution, global warming and other problems, and thus meet people's demand for renewable energy. Electrochemical water splitting, as an environmentally friendly method, is an ideal way to produce clean, high-purity hydrogen fuel. The efficient production of hydrogen mainly depends on the activity and cost of the electrocatalyst. Platinum and its alloys are recognized as the best catalysts for the hydrogen evolution reaction. However, the low reserves and high cost of platinum have severely limited its large-scale application. Therefore, people have been committed to exploring alternative materials for non-precious metal catalysts, including transition metal chalcogenides and carbides and their derivatives.
[0003] Tungsten carbide has a d-band electronic structure similar to that of platinum metal and can efficiently undergo hydrogen evolution reaction, so it is one of the most likely candidate compounds to replace platinum-based precious metals. However, it is easy to sinter into blocks at high temperatures, which greatly reduces the effective surface area. Due to the lack of suitable precursors to uniformly hybridize the tungsten source and the carbon source to form an ordered nanostructure, it is still a huge challenge to synthesize tungsten carbide nanostructures with high specific surface area through simple preparation methods. Therefore, further research and optimization of the preparation method and catalytic performance of tungsten carbide catalysts are urgently needed. Summary of the invention
[0004] According to one aspect of the present application, a tungsten carbide-tungsten sulfide composite catalytic material is provided. The composite material uses tungsten foil as a substrate and a tungsten source, so that a stable chemical bond can be formed between the tungsten carbide-tungsten sulfide film and the tungsten foil interface, thereby enhancing the conductivity; a tungsten trioxide film is formed on the tungsten foil. Using tungsten trioxide as a precursor, the tungsten carbide-tungsten sulfide film synthesized in one step has a vertical flaky structure, which increases the specific surface area and thereby increases the number of active sites of the catalyst.
[0005] A tungsten carbide-tungsten sulfide composite catalytic material, comprising a tungsten foil substrate layer and a tungsten carbide-tungsten sulfide composite catalytic layer;
[0006] The tungsten carbide-tungsten sulfide composite catalyst layer grows on the surface of the tungsten foil base layer.
[0007] Optionally, the tungsten carbide-tungsten sulfide composite catalytic layer covers the surface of the tungsten foil base layer.
[0008] Optionally, the tungsten carbide-tungsten sulfide composite catalyst layer is in the form of a vertical flaky film.
[0009] Optionally, the specific surface area of the tungsten carbide-tungsten sulfide composite catalyst material is 0.1 cm 2 ~10cm 2 .
[0010] Optionally, the specific surface area of the tungsten carbide-tungsten sulfide composite catalytic material is independently selected from 0.1m 2 、0.2m 2 、0.4m 2 、0.6m 2 、0.8m 2 , 1m 2 , 2m 2 、3m 2 、4m 2 、5m 2 、6m 2 、7m 2 、8m 2 、9m 2 、10m 2 Any value in or any range between them.
[0011] Optionally, in the tungsten carbide-tungsten sulfide composite catalyst layer, the molar ratio of tungsten carbide to tungsten sulfide is 5:1 to 1:1.
[0012] Optionally, the molar ratio of tungsten carbide to tungsten sulfide is independently selected from any value of 5:1, 4:1, 3:1, 2:1, 1:1, or any range therebetween.
[0013] According to another aspect of the present application, a method for preparing a tungsten carbide-tungsten sulfide composite catalytic material is provided. The preparation method adopts a chemical vapor deposition method, and has simple operation, low cost, and is easy to mass produce.
[0014] A method for preparing a tungsten carbide-tungsten sulfide composite catalytic material comprises the following steps:
[0015] (S1) Reaction I on tungsten foil to obtain tungsten trioxide film;
[0016] (S2) placing a sulfur source upstream of the circulating carbon source gas and a tungsten trioxide film reaction II downstream to obtain a tungsten carbide-tungsten sulfide composite catalytic material.
[0017] Optionally, the sulfur source is sulfur powder.
[0018] Optionally, the mass of the sulfur source is 0.05g to 0.2g.
[0019] Optionally, the conditions for reaction I are as follows:
[0020] The insulation temperature is 700℃~900℃;
[0021] The time is 10min to 30min.
[0022] Optionally, the heating rate is 15°C / min to 20°C / min.
[0023] Optionally, the holding temperature is independently selected from any value of 700° C., 750° C., 800° C., 850° C., 900° C., or any range therebetween.
[0024] Optionally, the heating rate is independently selected from any value of 15°C / min, 16°C / min, 17°C / min, 18°C / min, 19°C / min, 20°C / min, or any range therebetween.
[0025] Optionally, the time is independently selected from any value among 10 min, 15 min, 20 min, 25 min, 30 min, or any range between them.
[0026] Optionally, the reaction atmosphere is a mixture of oxygen and argon;
[0027] The flow ratio of oxygen to argon is 1:9 to 1:4.
[0028] Optionally, the flow rate of oxygen is 10 sccm to 20 sccm.
[0029] Optionally, the flow ratio of oxygen to argon is independently selected from any value of 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, or any range therebetween.
[0030] Optionally, the conditions of reaction II are as follows:
[0031] The upstream insulation temperature is 150℃~200℃;
[0032] The heating rate is 3℃ / min~5℃ / min.
[0033] Optionally, the upstream insulation temperature is independently selected from any value of 150° C., 160° C., 170° C., 180° C., 190° C., 200° C., or any range therebetween.
[0034] Optionally, the heating rate is independently selected from any value of 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, or any range therebetween.
[0035] Optionally, the downstream insulation temperature is 800°C to 1000°C;
[0036] The heating rate is 20℃ / min~30℃ / min.
[0037] Optionally, the downstream insulation temperature is independently selected from any value of 800° C., 850° C., 900° C., 950° C., 1000° C., or any range therebetween.
[0038] Optionally, the heating rate is independently selected from any value of 20°C / min, 22°C / min, 24°C / min, 26°C / min, 28°C / min, 30°C / min, or any range therebetween.
[0039] Optionally, the insulation time is 10 min to 30 min.
[0040] Optionally, the holding time is independently selected from any value among 10 min, 15 min, 20 min, 25 min, 30 min, or any range value therebetween.
[0041] Optionally, the carbon source gas is selected from one of methane, acetylene and carbon monoxide.
[0042] Optionally, the atmosphere of reaction II is a mixture of argon and hydrogen, wherein:
[0043] The argon gas flow rate is 10 sccm to 50 sccm;
[0044] The hydrogen flow rate is 10 sccm to 50 sccm.
[0045] Optionally, the argon flow rate and the hydrogen flow rate are independently selected from any value of 10 sccm, 15 sccm, 20 sccm, 25 sccm, 30 sccm, 35 sccm, 40 sccm, 45 sccm, 50 sccm, or any range therebetween.
[0046] The beneficial effects of this application include:
[0047] 1) The present application provides a tungsten carbide-tungsten sulfide composite catalytic material, which uses tungsten foil as a substrate and tungsten source, so that the tungsten carbide-tungsten sulfide film and the tungsten foil interface can form a stable chemical bond, thereby enhancing the conductivity; a tungsten trioxide film is formed on the tungsten foil, and tungsten trioxide is used as a precursor. The tungsten carbide-tungsten sulfide film synthesized in one step has a vertical flaky structure, which increases the specific surface area and thereby increases the number of active sites of the catalyst.
[0048] 2) The preparation method provided in the present application adopts chemical vapor deposition, which has the advantages of simple operation, low cost and easy mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 Scanning electron microscope images of tungsten trioxide and tungsten sulfide films prepared in Example 1 of the present application.
[0050] Figure 2 This is a scanning electron microscope image of the tungsten carbide film prepared in Example 2 of the present application.
[0051] Figure 3 This is a scanning electron microscope image of the tungsten carbide-tungsten sulfide composite catalytic material prepared in Example 3 of the present application.
[0052] Figure 4 X-ray diffraction patterns of tungsten sulfide, tungsten carbide and tungsten carbide-tungsten sulfide composite catalytic materials prepared in Examples 1 to 3 of the present application.
[0053] Figure 5 LSV (Linear Sweep Voltammetry) curves of hydrogen evolution from electrolysis of water of tungsten sulfide, tungsten carbide and tungsten carbide-tungsten sulfide composite catalytic materials prepared in Examples 1 to 3 of the present application.
[0054] Figure 6 This is the Tafel plot (Tafel slope) curve of hydrogen evolution by electrolysis of water of tungsten sulfide, tungsten carbide and tungsten carbide-tungsten sulfide composite catalytic materials prepared in Examples 1 to 3 of the present application.
[0055] Figure 7 These are the EIS (electrochemical impedance spectroscopy) curves of hydrogen evolution by electrolysis of water of tungsten sulfide, tungsten carbide and tungsten carbide-tungsten sulfide composite catalytic materials prepared in Examples 1 to 3 of the present application.
[0056] Figure 8 Electrochemical double-layer capacitance diagram of water electrolysis and hydrogen evolution of tungsten sulfide, tungsten carbide and tungsten carbide-tungsten sulfide composite catalytic materials prepared in Examples 1 to 3 of the present application.
[0057] Fig. 9 This is the stability curve of hydrogen evolution in water electrolysis of the tungsten carbide-tungsten sulfide composite catalytic material prepared in Example 3 of the present application. DETAILED DESCRIPTION
[0058] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0059] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0060] The analysis method in the examples of this application is as follows:
[0061] Scanning electron microscopy (Zeiss FE-SEM Sigma300) was used for electron microscopy analysis.
[0062] XRD analysis was carried out using an X-ray powder diffractometer (Miniflex 600).
[0063] The electrochemical performance was analyzed using an electrochemical workstation (CHI 660e).
[0064] Example 1
[0065] Step 1: Prepare a tungsten trioxide film on the tungsten foil. The film has an uneven surface and forms a stable chemical bond with the tungsten foil interface, which can enhance conductivity. As a precursor for the subsequent catalytic layer preparation, the specific preparation method is as follows:
[0066] The tungsten foil with a purity of 99.95% and a thickness of 0.1mm was cut into 1×1cm specifications and soaked in dilute hydrochloric acid for 30 minutes to remove the surface oxide layer, and then the surface oil was removed by boiling acetone, and then ultrasonically cleaned three times in ultrapure water and anhydrous ethanol in turn, and the cleaning time was 30 minutes. Finally, the cleaned tungsten foil was dried in nitrogen and placed in a tube furnace. The tube furnace was sealed, and a part of the air in the furnace was evacuated until the vacuum reading was 0.2atm, and a part of the air was retained. Then, argon was filled to the normal pressure of 1atm, and the tube furnace was sealed again; the tube furnace was heated to 800 degrees at a heating rate of 20℃ / min, and the temperature was maintained for 10 minutes. During the entire heating and calcination process, a part of the gas was released when the pressure was higher than 1atm and then sealed, so that the entire process was always in a state of 1atm and air (oxygen) was prevented from entering. Cool to room temperature to obtain a tungsten trioxide film on the tungsten foil.
[0067] Step 2: Prepare tungsten sulfide film. The specific preparation method is as follows:
[0068] The prepared tungsten trioxide film is placed in the downstream temperature zone of a vacuum tube furnace, and the sulfur source is placed in the upstream temperature zone of the tube furnace. In an argon and hydrogen atmosphere of 20 sccm, the upstream temperature zone of the tube furnace is heated to 200°C at a heating rate of 4°C / min, and the downstream temperature zone is rapidly heated to 900°C at a heating rate of 22°C / min, and the reaction temperature is maintained for 20 minutes, and then naturally cooled to room temperature to obtain a tungsten sulfide film.
[0069] The obtained tungsten trioxide and tungsten sulfide films were analyzed by field emission scanning electron microscope. Figure 1 As shown, the morphology of tungsten sulfide is similar to that of tungsten trioxide, showing dense stones and an uneven surface, but the tungsten sulfide blocks are larger than those of tungsten trioxide.
[0070] Example 2
[0071] Step 1: Prepare a tungsten trioxide film on a tungsten foil, which is consistent with the preparation method of step 1 in Example 1.
[0072] Step 2: Prepare tungsten carbide film on tungsten foil. The specific preparation method is as follows:
[0073] The prepared tungsten trioxide film is placed in a clean ceramic boat, placed in the heating zone of a tube furnace, sealed and evacuated to exhaust the air in the tube furnace, then argon is introduced to clean the tube furnace and the furnace pressure reaches 1atm, the vent valve is opened, and the tube furnace is heated to 800 degrees within 40 minutes in an atmosphere with argon and hydrogen gas flow rates of 70sccm and 30sccm respectively. When the temperature rises to 800 degrees, methane is introduced with a flow rate of 15sccm, and the insulation time is 20 minutes. When the insulation is completed, methane and hydrogen are turned off. After naturally cooling to room temperature, a tungsten carbide catalytic material is obtained.
[0074] The obtained tungsten carbide film was subjected to field emission scanning electron microscopy morphology analysis. Figure 2 As shown, tungsten carbide is easy to sinter into blocks, which reduces the specific surface area and is not conducive to improving the catalytic performance.
[0075] Example 3
[0076] Step 1: Prepare a tungsten trioxide film on a tungsten foil, which is consistent with the preparation method of step 1 in Example 1 and Example 2.
[0077] Step 2: Prepare a tungsten carbide-tungsten sulfide composite film on tungsten foil. The specific preparation method is as follows:
[0078] The tungsten trioxide film is placed in the downstream temperature zone of the tube furnace, 0.1g of sulfur powder is placed in the upstream temperature zone of the tube furnace, and the air in the tube furnace is exhausted by sealing and vacuuming. Then, argon gas is introduced to clean the tube furnace and the furnace pressure reaches 1atm. The vent valve is opened, the argon flow rate is reduced to 20sccm, and 20sccm of hydrogen is introduced; the upstream temperature zone is raised to 200°C at a heating rate of 4°C / min, and the downstream temperature zone of the tube furnace is heated to 900 degrees at a heating rate of 22°C / min. When the temperature rises to 800 degrees, methane is introduced at a flow rate of 40sccm, and the insulation time is 20 minutes. When the insulation is completed, methane and hydrogen are turned off. Then it is naturally cooled to room temperature to obtain a tungsten carbide-tungsten sulfide composite catalytic material.
[0079] The obtained tungsten carbide-tungsten sulfide composite catalyst material was subjected to field emission scanning electron microscopy morphology analysis. Figure 3 As shown, tungsten carbide-tungsten sulfide is a vertical nano-flake film with a greatly increased specific surface area and can also expose more edge sites, which is beneficial to the improvement of catalytic performance.
[0080] The tungsten sulfide film obtained in Example 1, the tungsten carbide film obtained in Example 2, and the tungsten carbide-tungsten sulfide film obtained in Example 3 were analyzed by X-ray diffraction. Figure 4 As shown, the phases of tungsten carbide and tungsten sulfide can be detected simultaneously in the tungsten carbide-tungsten sulfide film, proving the existence of the composite material of tungsten carbide and tungsten sulfide film.
[0081] The electrocatalytic hydrogen evolution performance of tungsten sulfide, tungsten carbide and tungsten carbide-tungsten sulfide films obtained in Examples 1, 2 and 3, respectively, was studied. The performance was measured using a three-electrode system, with the reference electrode being an Ag / AgCl electrode (with a saturated KCl solution as the internal electrolyte), the carbon rod being the counter electrode, and 0.5MH2SO4 being the electrolyte. The above tungsten-based samples were cut into a certain size and fixed to a clip electrode (Pt sheet as a conductor) as a working electrode, and then tested on an electrochemical workstation (CHI600E, Shanghai Chenhua Company). The test results in the present invention are based on the formula: E RHE =E Ag / AgCl +0.059×PH+0.198, normalize the current density and potential value respectively. Before the test, argon gas was introduced for half an hour to purify the electrolyte to remove adsorbed O2. The scanning rate of the linear polarization curve was 2mV / s, and the scanning range was 0V~-0.5V vs.RHE. The stability of the catalyst was measured by cyclic voltammetry (CV) with a scanning rate of 100mV / s and a voltage range of 0V~-0.6Vvs.RHE. Electrochemical impedance spectroscopy (EIS) measurements were performed on the same device at a frequency of 1000Hz to 0.01Hz. Electrochemical double layer capacitance (C dl ) is used to measure the effective surface area of the catalytic material, which can be characterized by measuring the non-Faraday capacitive current related to the charging of the double-layer capacitor. The larger the value, the more active sites involved in the hydrogen evolution reaction. In the present invention, it is determined by the scan rate of the cyclic voltammetry curve. The geometric area used for the measurement in the present invention is 1 cm 2 .
[0082] The present invention measures the activity of the electrocatalytic hydrogen evolution reaction by five commonly used tests, namely, overpotential (current density of 10 mA / cm 2 The corresponding voltage when , Tafel slope, impedance, electrochemical double layer capacitance and stability.
[0083] Figure 5 The polarization curves of tungsten sulfide, tungsten carbide and tungsten carbide-tungsten sulfide composite catalyst in 0.5MH2SO4 are shown. It can be seen that the tungsten carbide-tungsten sulfide composite catalyst only needs an overpotential of 68mV to reach 10mA / cm 2 The cathode current density of Figure 6 As shown, j is the current density. The Tafel slope of the tungsten carbide-tungsten sulfide composite catalyst material is 56mV / dec, which is much smaller than that of tungsten sulfide and tungsten carbide films, indicating that the rate of hydrogen production is the fastest. Its value also shows that the rate-limiting step of the hydrogen evolution reaction is the desorption process of hydrogen. Figure 7The impedance of tungsten carbide-tungsten sulfide composite catalyst material is the smallest, indicating that the composite material has good electron transport ability. Figure 8 This is the electrochemical double layer capacitance diagram. It can be seen from the figure that the tungsten carbide-tungsten sulfide composite catalytic material has the largest effective surface area, indicating that the composite material has a rich number of active sites. Fig. 9 The cyclic stability test of tungsten carbide-tungsten sulfide composite catalytic material shows that after 2000 CV cycles, the performance of the composite material has not decayed at all, indicating that the tungsten carbide-tungsten sulfide electrode has excellent stability.
[0084] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a tungsten carbide-tungsten sulfide composite catalytic material, It is characterized in that The following steps are involved: (S1) Reaction I on tungsten foil to obtain tungsten trioxide film; (S2) placing a sulfur source upstream of the circulating carbon source gas and a tungsten trioxide film reaction II downstream to obtain a tungsten carbide-tungsten sulfide composite catalytic material; The conditions for reaction I are as follows: The insulation temperature is 700℃~900℃; The time is 10 min~30 min; The reaction atmosphere is a mixture of oxygen and argon; The flow ratio of oxygen and argon is 1:9~1:4; The conditions for reaction II are as follows: The upstream insulation temperature is 150℃~200℃; The heating rate is 3 ℃ / min ~5 ℃ / min; The downstream insulation temperature is 800℃~1000℃; The heating rate is 20 ℃ / min ~30 ℃ / min; The atmosphere of reaction II is a mixture of argon and hydrogen, wherein: The argon flow rate is 10 sccm~50 sccm; The hydrogen flow rate is 10 sccm~50 sccm; The tungsten carbide-tungsten sulfide composite catalytic material comprises a tungsten foil substrate layer and a tungsten carbide-tungsten sulfide composite catalytic layer; The tungsten carbide-tungsten sulfide composite catalyst layer is grown on the surface of the tungsten foil substrate layer; The tungsten carbide-tungsten sulfide composite catalyst layer is in the form of a vertical scale film.
2. The preparation method according to claim 1, It is characterized in that The tungsten carbide-tungsten sulfide composite catalyst layer covers the surface of the tungsten foil base layer.
3. The preparation method according to claim 1, It is characterized in that In the tungsten carbide-tungsten sulfide composite catalyst layer, the molar ratio of tungsten carbide to tungsten sulfide is 5:1 to 1:
1.
4. The preparation method according to claim 1, It is characterized in that The sulfur source is sulfur powder.
5. The preparation method according to claim 1, It is characterized in that The mass of the sulfur source is 0.05 g to 0.2 g.
6. The preparation method according to claim 1, It is characterized in that The carbon source gas is selected from one of methane, acetylene and carbon monoxide.
7. The preparation method according to claim 1, It is characterized in that The heating rate of the reaction I is 15°C / min to 20°C / min.
8. The preparation method according to claim 1, It is characterized in that The insulation time of the reaction II is 10 min to 30 min.
9. Use of the tungsten carbide-tungsten sulfide composite catalytic material obtained by the preparation method according to any one of claims 1 to 8 as a hydrogen evolution catalyst.
Citation Information
Cited By
Preparation method and application of tungsten-molybdenum carbide nanosheet heterojunction catalyst
CN118880388B