Anode catalyst layer of proton exchange membrane electrolyzed water membrane electrode based on aggregate structure regulation and control as well as preparation and application of anode catalyst layer
By using self-assembly technology of nitrogen thiol and IrOx nanocatalysts in the proton exchange membrane electrode anode catalytic layer, the problem of high transport resistance of dissolved and bubble oxygen caused by dense agglomerates is solved, and low transmission is achieved The electrolytic performance of polarization and high electrolytic currents has improved, reducing the cost of electrolytic hydrogen production.
Patent Information
- Application Number
- CN202411084730.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
AI Technical Summary
The dense agglomerate structure on the anode side of the proton exchange membrane water electrolysis (PEMFC) leads to high transport resistance of dissolved oxygen and poor transport of bubble oxygen, resulting in high transmission overpotential loss, limiting the reduction of the cost of electrolytic hydrogen production.
By introducing self-assembly technology of nitrogen thiol and IrOx nanocatalysts into the catalytic layer of the proton exchange membrane electrode, the agglomerate structure is regulated, and the catalyst-ionomer agglomerate structure is optimized by the sacrificial template method to improve dissolved oxygen and bubble oxygen transmission efficiency.
It significantly reduces the transmission overpotential loss under high electrolytic hydrogen production current, improves the catalyst utilization rate, reduces the cost of electrolytic hydrogen production, and improves the electrolytic performance.
Smart Images

Figure CN118932383A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a water electrolysis hydrogen production membrane electrode and a preparation method thereof, and in particular to an anode catalyst layer of a proton exchange membrane water electrolysis membrane electrode based on aggregate structure regulation and a preparation method thereof. Background Art
[0002] Proton exchange membrane water electrolysis (PEMFC) is a clean and efficient hydrogen production technology. However, due to the overpotential of the anode side at high electrolysis current, its hydrogen production cost has remained high, which is the fundamental reason why this technology cannot be further popularized. Among them, the transmission overpotential loss, which increases at an accelerated rate with the increase of electrolysis current, is the main source of overpotential loss under high electrolysis hydrogen production current. The rapidly rising transmission overpotential loss comes from two aspects. On the one hand, it comes from the large accumulation of local dissolved oxygen concentration inside the dense agglomerates. The oxygen released on the anode side first accumulates in the catalyst-ionomer agglomerates. Because the agglomerate structure is too dense, the transmission distance of dissolved oxygen in the agglomerates is too long. As the electrolysis hydrogen production current increases, this local accumulation of dissolved oxygen concentration becomes more serious, causing the transmission overpotential to rise; on the other hand, it comes from the tight coating of the ionomer on the surface of the agglomerate, which makes the oxygen bubble nucleation sites in the anode catalyst layer very few, and it is impossible to achieve good oxygen transmission. That is to say, the poor dissolved oxygen transport and bubble oxygen transport in the anode catalyst layer caused by the special catalyst-aggregate structure are the fundamental reasons for the high transport overpotential loss at large electrolysis hydrogen production current.
[0003] Chinese patent application CN202311011120.7 discloses the use of special morphology optimization of the electrolytic cell flow channel to achieve transmission optimization on both sides of the electrolytic hydrogen production membrane electrode. Although this solution can improve the electrolysis efficiency by optimizing the transmission loss on both sides of the anode and cathode, this solution is a transmission overpotential optimization based on the flow channel device design. This solution requires improving the processing accuracy of the flow channel, which greatly increases the processing cost of the flow channel compared to the traditional flow channel design solution, and increases the transmission distance of the reactants and products. Although the transmission loss is reduced, the flow loss along the way is also increased accordingly, which increases the pump power consumption.
[0004] Chinese patent CN202210467407.X discloses a special microfiber structure that directly regulates oxygen bubbles in the electrolyte, and optimizes the electrolytic performance by means of the aggregation behavior between bubbles. However, this solution is also a system-scale bubble optimization work, the purpose of which is to achieve rapid separation of microbubbles. This solution increases the complexity of the electrolysis system, increases the flow distance of the product, increases the power consumption of the pump, and does not regulate the root cause of the higher transmission overpotential-the unreasonable catalyst-ionomer agglomerate structure. It is only an optimization work at the system optimization level. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a proton exchange membrane electrolysis water membrane electrode anode catalyst layer based on agglomerate structure regulation and a preparation method thereof, so as to solve the problem that the anode side of the proton exchange membrane electrolysis water membrane electrode has too high transmission resistance of the precipitated dissolved oxygen inside the agglomerate due to the overly dense structure of the basic unit catalyst-ionomer agglomerate constituting it; and the problem that the tight coating of the agglomerate by the ionomer causes insufficient nucleation sites for bubble oxygen, making it difficult to achieve efficient oxygen transmission, thereby causing the anode transmission resistance to rise rapidly with the increase of the electrolysis current, and the cost of hydrogen production by electrolysis cannot be further reduced.
[0006] The object of the present invention can be achieved by the following technical scheme: a method for preparing an anode catalyst layer of a proton exchange membrane water electrolysis membrane electrode based on aggregate structure regulation, the method comprising the following steps:
[0007] (1) mixing n-octadecyl mercaptan and deionized water uniformly to prepare a self-assembly solution A;
[0008] (2) placing IrOx nanocatalyst particles in self-assembly solution A to obtain catalyst-self-assembly solution B, stirring, ultrasonicating, centrifuging, and washing to obtain solid particles;
[0009] (3) drying the solid particles obtained in step (2) to obtain catalyst-ODT self-assembled solid particles C;
[0010] (4) adding the catalyst-ODT self-assembled solid particles C and the perfluorosulfonic acid ionomer solution to the dispersed solution and mixing them to obtain an anode catalyst slurry D;
[0011] (5) Spray the anode catalyst slurry D onto one side of the proton exchange membrane and dry it to obtain the anode catalyst layer.
[0012] Furthermore, the mass concentration of the self-assembly solution A in step (1) is (0.5-4)%.
[0013] Furthermore, the mass volume ratio of the IrOx nanocatalyst described in step (2) to the self-assembly solution A is (50-100) mg / mL.
[0014] Furthermore, the drying temperature in step (3) does not exceed 40°C.
[0015] Furthermore, the dispersion solution described in step (4) is a mixture of ultrapure water and isopropanol in a volume ratio of 10:1-10:7.
[0016] Furthermore, the mass ratio of the catalyst-ODT self-assembled solid particles C, the perfluorosulfonic acid ionomer solution and the dispersed solution in step (4) is 1.6:1:500-1.6:1:100.
[0017] Furthermore, in step (4), each material is ultrasonically treated in a water bath not exceeding 20° C. for 12-36 hours to obtain an ultrasonically uniform anode catalyst slurry D.
[0018] The present invention also provides a proton exchange membrane water electrolysis membrane electrode anode catalyst layer prepared by the above preparation method.
[0019] The present invention also provides an application of an anode catalyst layer of a proton exchange membrane water electrolysis membrane electrode, and the anode catalyst layer is applied to the proton exchange membrane water electrolysis membrane electrode.
[0020] The proton exchange membrane water electrolysis membrane electrode is prepared by spraying anode catalyst slurry and cathode catalyst slurry on a proton exchange membrane and on both sides thereof, respectively, and drying them.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] (1) The present invention directly regulates the structure of the agglomerates that is not conducive to the transmission of dissolved oxygen and bubble oxygen. Without changing the catalyst system, the slurry preparation process and the catalytic activity, a good agglomerate structure is obtained by means of the sacrificial template method. The agglomerate regulation method on the anode side of the membrane electrode based on the sacrificial template method directly designs and optimizes the structure near the anode triple phase point that causes excessive oxygen transmission resistance, thereby alleviating the problem of high transmission overpotential caused by the accumulation of dissolved oxygen concentration inside the agglomerates and poor bubble oxygen management, so as to achieve the design and development of the anode catalyst layer of the membrane electrode for electrolysis of water with low transmission polarization, low loading and high electrolysis current, which greatly reduces the transmission overpotential loss under high electrolysis hydrogen production current density, improves catalyst utilization and reduces hydrogen production costs.
[0023] (2) The present invention optimizes the anode side dissolved oxygen and bubble oxygen transmission by optimizing the agglomerate structure in the anode catalyst layer of the proton exchange membrane electrolysis membrane electrode, reduces the anode transmission overpotential, and ultimately improves the electrolysis performance and significantly reduces the cost of water electrolysis. The method is mainly used for the preparation of proton exchange membrane electrolysis membrane electrodes, slurry design and other related fields. The core technology is: based on the traditional slurry preparation method and the nanoparticle IrOx catalyst system, an organic self-assembly method is directly added in the slurry preparation process to regulate the agglomerate morphology and structural characteristics, and the morphology of the dense catalyst-ionomer agglomerate structure is controlled by means of the in-situ electrochemical removal of the sacrificial template method, thereby improving the high resistance transmission of dissolved oxygen-bubble oxygen inside the agglomerate structure, while reducing the mutual coverage inside the catalyst clusters to increase the number of catalyst active sites, thereby significantly improving the electrolysis performance and reducing the cost of hydrogen production by electrolysis.
[0024] (3) The method of the present invention is suitable for optimizing the structure and performance of the anode of the membrane electrode of proton exchange membrane water electrolysis, and is realized by coordinating with a targeted slurry design scheme. It has the following effects:
[0025] a) The present invention can directly add a step of organic self-assembly process to the original PEM water electrolysis hydrogen production membrane electrode anode catalyst system and slurry system to carry out targeted agglomerate structure and morphology regulation, without the need for complex process system development and trial and error, to achieve improved electrolysis performance;
[0026] b) The present invention directly performs targeted regulation based on the structure and morphology of the anode-side agglomerates, does not rely on complex device design and system design, and simultaneously optimizes and improves the dissolved oxygen transmission resistance in the agglomerates, the bubble oxygen transmission behavior in the catalyst layer, and the catalyst utilization rate in the anode catalyst layer;
[0027] c) Optimizing the transmission loss overpotential on the anode side of the water electrolysis membrane electrode in conjunction with this method can greatly increase the operating current of the hydrogen electrolysis membrane electrode and improve the catalyst utilization rate without affecting the catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 : are electron microscope images of catalyst particles, wherein a is the agglomeration of catalyst particles without regulation in Comparative Example 1, and b is the agglomeration of catalyst particles after regulation obtained in Example 1;
[0029] Figure 2 : are electron microscope images of the catalyst-ionomer secondary agglomeration, wherein a is the unregulated catalyst-ionomer secondary agglomeration of Comparative Example 1, and b is the regulated catalyst-ionomer secondary agglomeration obtained in Example 1;
[0030] Figure 3 are electron microscope images of the catalytic layer, wherein a is an electron microscope image of the catalytic layer of Comparative Example 1, and b is an electron microscope image of the catalytic layer obtained in Example 1;
[0031] Figure 4 ORE test voltage and current density diagram of the catalyst layer ECSA before and after regulation in Example 1 and Comparative Example 1;
[0032] Figure 5 The ORE agglomeration performance diagram of the catalyst layer ECSA before and after regulation of Example 1 and Comparative Example 1;
[0033] Figure 6 This is a diagram of the water point hydrolysis performance of the membrane electrode obtained in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0035] The method for preparing a proton exchange membrane water electrolysis membrane electrode based on aggregate structure regulation of the present invention comprises the following steps:
[0036] (1) A 0.5-4% octadecyl mercaptan (ODT) solution (ODT mixed with anhydrous ethanol) was prepared as a self-assembly solution A, and after ultrasonication for 10 minutes, the solution was allowed to stand for 24 hours to ensure that the solution was completely mixed and no flocculent sediment was visible to the naked eye.
[0037] (2) placing commercially available IrOx nanocatalyst particles in the self-assembly solution A prepared in step (1) to obtain a catalyst-self-assembly solution B (wherein the mass volume ratio of the commercially available IrOx nanocatalyst particles to the self-assembly solution A is 50-100 mg / mL), subjecting the catalyst-self-assembly solution B to magnetic stirring at room temperature not exceeding 20° C. for a stirring time of not less than 24 hours, and subjecting the obtained solution to multiple ultrasonic-centrifugation-washing operations until the supernatant obtained by centrifugation is completely clarified.
[0038] (3) The solid particles obtained in step (2) are placed in a vacuum oven for drying, and the drying temperature is ensured not to exceed 40° C. After overnight drying, catalyst-ODT self-assembled solid particles C are obtained.
[0039] (4) The catalyst-ODT self-assembled solid particles C, 20% concentration of commercially available perfluorosulfonic acid (PFSA) ionomer solution, and a dispersion solution consisting of ultrapure water and isopropanol in a volume ratio of (10:1-20:1) are mixed to obtain a slurry solution, wherein the mass ratio of the catalyst-ODT self-assembled solid particles C, the perfluorosulfonic acid (PFSA) ionomer solution and the dispersion solution is (1.6:1:500-1.6:1:100), and the obtained mixed solution is ultrasonically treated in a water bath not exceeding 20°C for 24 hours to obtain an ultrasonically uniform anode catalyst slurry D.
[0040] A certain mass of solid particles of a commercially available Pt / C catalyst, a 20% concentration of a commercially available PFSA ionomer solution, and a dispersion solution consisting of ultrapure water and isopropanol in a mass ratio of (5:2-5:4) are mixed to obtain a slurry solution, wherein the mass ratio of the Pt / C catalyst, the perfluorosulfonic acid (PFSA) ionomer solution, and the dispersion solution is (2.5:1:625-2.5:1:100), and the resulting mixed solution is ultrasonically subjected to a water bath not exceeding 20°C for 24 hours to obtain an ultrasonically uniform cathode catalyst slurry E.
[0041] (5) The anode catalyst slurry D and the cathode catalyst slurry E were sprayed on both sides of the pretreated commercially available Nafion 115 proton exchange membrane using an ultrasonic spraying device, and the membrane electrode was dried at room temperature for not less than 4 hours to obtain a membrane electrode F.
[0042] (6) Assemble the membrane electrode F in the electrolytic cell test fixture, apply a 1.0-1.5V cyclic potential scan test to the anode until the peak area no longer changes.
[0043] (7) Activate the battery according to the standard activation procedure for the electrolytic cell, and then perform a standard electrolytic cell performance test.
[0044] The various raw materials and equipment used in the present invention are all commercially available raw materials and conventional equipment in the art. For example, the commercially available Pt / C catalyst used in the present application is TEC10E50E.
[0045] Example 1
[0046] (1) A 1.0% octadecyl mercaptan (ODT) solution (prepared by mixing ODT with anhydrous ethanol) was prepared as self-assembly solution A, and after ultrasonication for 10 minutes, the solution was allowed to stand for 24 hours to ensure that the solution was completely mixed and no flocculent sediment was visible to the naked eye.
[0047] (2) placing commercially available IrOx nanocatalyst particles in the self-assembly solution A prepared in step (1) to obtain a catalyst-self-assembly solution B (wherein the mass volume ratio of the commercially available IrOx nanocatalyst particles to the self-assembly solution A is 50 mg / mL), subjecting the catalyst-self-assembly solution B to magnetic stirring at room temperature not exceeding 20° C. for a stirring time of not less than 24 hours, and subjecting the obtained solution to multiple ultrasonic-centrifugation-washing operations until the supernatant obtained by centrifugation is completely clarified.
[0048] (3) The solid particles obtained in step (2) are placed in a vacuum oven for drying, and the drying temperature is ensured not to exceed 40° C. After overnight drying, catalyst-ODT self-assembled solid particles C are obtained.
[0049] (4) The catalyst-ODT self-assembled solid particles C, 20% concentration of commercially available perfluorosulfonic acid (PFSA) ionomer solution, and a dispersion solution consisting of ultrapure water and isopropanol in a mass ratio of 10:1 are mixed to obtain a slurry solution, wherein the mass ratio of the catalyst-ODT self-assembled solid particles C, the perfluorosulfonic acid (PFSA) ionomer solution, and the dispersion solution is 1.6:1:500. The obtained mixed solution is ultrasonically treated in a water bath not exceeding 20°C for 24 hours to obtain an ultrasonically uniform anode catalyst slurry D.
[0050] A certain mass of solid particles of a commercially available Pt / C catalyst (TEC10E50E), a 20% concentration of a commercially available PFSA ionomer solution, and a dispersion solution consisting of ultrapure water and isopropanol in a mass ratio of 10:1 are mixed to obtain a slurry solution, wherein the mass ratio of the Pt / C catalyst (TEC10E50E), the perfluorosulfonic acid (PFSA) ionomer solution, and the dispersion solution is 2.5:1:625, and the resulting mixed solution is ultrasonically subjected to a water bath not exceeding 20°C for 24 hours to obtain an ultrasonically uniform cathode catalyst slurry E.
[0051] (5) The anode catalyst slurry D and the cathode catalyst slurry E were sprayed on both sides of the pretreated commercially available Nafion 117 proton exchange membrane using an ultrasonic spraying device, and the membrane electrode was dried at room temperature for not less than 4 hours to obtain a membrane electrode F.
[0052] (6) Assemble the membrane electrode F in the electrolytic cell test fixture, apply a 1.0-1.5V cyclic potential scan test to the anode until the peak area no longer changes.
[0053] (7) Activate the battery according to the standard activation procedure for the electrolytic cell, and then perform a standard electrolytic cell performance test.
[0054] Comparative Example 1
[0055] The method for preparing a proton exchange membrane water electrolysis membrane electrode comprises the following steps:
[0056] (1) Commercially available IrOx nanocatalyst particles, 20% concentration of commercially available PFSA ionomer solution, and a dispersion solution consisting of ultrapure water and isopropanol in a mass ratio of 10:1 are mixed to obtain a slurry solution, wherein the mass ratio of the commercially available IrOx nanocatalyst particles, the PFSA ionomer solution, and the dispersion solution is 1.6:1:500, and the slurry solution is ultrasonically treated in a water bath not exceeding 20° C. for 24 hours to obtain an ultrasonically uniform anode catalyst slurry.
[0057] A certain mass of solid particles of a commercially available Pt / C catalyst (TEC10E50E), a 20% concentration of a commercially available PFSA ionomer solution, and a dispersion solution consisting of ultrapure water and isopropanol in a mass ratio of 10:1 are mixed to obtain a slurry solution, wherein the mass ratio of the Pt / C catalyst (TEC10E50E), the PFSA ionomer solution, and the dispersion solution is 2.5:1:625. The obtained slurry solution is ultrasonically treated in a water bath not exceeding 20°C for 24 hours to obtain an ultrasonically uniform cathode catalyst slurry.
[0058] (2) The anode catalyst slurry and the cathode catalyst slurry were sprayed on both sides of the pretreated commercially available Nafion 117 proton exchange membrane by means of an ultrasonic spraying device, and the membrane electrode was dried at room temperature for not less than 4 hours to obtain a membrane electrode F.
[0059] (3) The membrane electrode F was assembled in the electrolytic cell test fixture, and a cyclic potential scanning test of 1.0-1.5 V was applied to the anode until the peak area no longer changed.
[0060] (4) Activate the battery according to the standard activation procedure for the electrolytic cell, and then perform a standard electrolytic cell performance test.
[0061] Performance testing:
[0062] (1) n-Octadecanethiol nano-self-assembly technology to achieve the morphology and structure control of the primary aggregates of the catalyst
[0063] In traditional catalyst slurries, IrOx catalyst solid particles will preferentially undergo the first agglomeration between solid particles due to their extremely high surface energy. In order to improve the catalytic activity of catalyst solid particles, these particles must be made extremely fine (usually 2-4nm), which leads to the van der Waals force between them driving these catalyst solid particles to form a very tight primary agglomeration structure. In this way, a large number of catalyst particles are shielded in the tight primary agglomerate structure, so that the active sites are covered and the catalyst utilization rate is extremely low;
[0064] The sulfur element in the ODT used in the present invention will preferentially form a chemical bond with the iridium element in the catalyst particles belonging to the platinum group metals. This chemical bond is stronger than the van der Waals force, so preferential adsorption between ODT and IrOx solid particles will occur. This preferential adsorption breaks the primary agglomeration behavior between IrOx particles, making the ODT-IrOx primary agglomeration structure significantly looser than the unmodified IrOx primary agglomeration. As shown in the attached Figure 1 As shown in a, it is a conventional catalyst slurry, i.e., the anode catalyst slurry prepared in comparative example 1. The unmodified IrOx primary agglomerates are small in size and very dense in structure, and the individual IrOx catalyst nano solid particles therein cannot be distinguished at all, and these primary agglomerates spontaneously form large-sized and dense catalyst secondary agglomerates; while the primary agglomerates modified by ODT in Example 1 have unchanged size, but very loose structure, and the IrOx catalyst nano solid particles with a diameter of 4 nm can be easily distinguished therein, and the surface of the primary agglomerates is covered with a layer of ODT organic film of uniform thickness (~20 nm), as shown in the attached Figure 1 As shown in b. This shows that the modification of the primary catalyst agglomerates by ODT greatly reduces the overlap rate between the catalyst particles within the agglomerates and improves the catalyst utilization rate;
[0065] (2) ODT self-assembled films as sacrificial templates achieve structural regulation of catalyst-ionomer secondary aggregates
[0066] As attached Figure 2As shown in a, in the electron microscope image of the side of the membrane electrode coated with the anode catalyst slurry in the unmodified traditional anode catalyst layer, i.e., comparative example 1, the sulfur element in the perfluorosulfonic acid ionomer will form a chemical bond with the iridium element in the primary agglomerate, and then tightly coat multiple IrOx primary agglomerates to form a dense secondary agglomerate structure. At the same time, the ionomer forms a dense 10-nanometer-thick film on the surface of the secondary agglomerate structure. On the one hand, the dense agglomerate structure makes it possible for the oxygen released from the catalytic active sites to be discharged first in the form of dissolved oxygen in the ionomer by diffusion over a long distance of concentration difference; on the other hand, the tight coating of the ionomer on the secondary agglomerate makes it extremely difficult to form defect sites in the secondary agglomerate that can provide oxygen bubble nucleation, resulting in extremely high resistance to oxygen bubble transmission in the anode catalyst layer;
[0067] As attached Figure 2 As shown in b, it is an electron microscope image of one side of the membrane electrode coated with the anode catalyst slurry prepared in Example 1. In the structurally optimized anode catalyst layer with the ODT self-assembled film as a sacrificial template, the originally spreading ODT self-assembled network is replaced by a multi-scale pore network spanning nanometers and micrometers. On the one hand, the formed pore network greatly shortens the transmission distance of dissolved oxygen in the secondary agglomerates and reduces the dissolved oxygen transmission resistance; on the other hand, the nano-micrometer multi-scale holes formed on the surface of the secondary agglomerates enhance the nucleation effect of oxygen bubbles, and a large number of oxygen bubble nucleation sites are formed near the secondary agglomerates, thereby optimizing the oxygen bubble transmission resistance inside the agglomerates.
[0068] (3) Enhanced oxygen transport and increased catalyst utilization have improved the performance of PEM electrolysis hydrogen production
[0069] As attached Figure 3 As shown, a is the electron microscope image of the anode side of the membrane electrode prepared in comparative example 1, and b is the electron microscope image of the anode side of the membrane electrode prepared in example 1. The bubble visualization characterization technology proves that the catalyst layer structure optimization achieved in the present invention does indeed enhance the oxygen bubble transmission near the catalyst layer.
[0070] Figure 4 ECSA detection graphs of the catalytic layers obtained in Example 1 (i.e., the catalytic layer prepared by the present invention in the figure) and Comparative Example 1 (i.e., the traditional catalytic layer in the figure), the detection method is: the PEMWE membrane electrodes prepared in Example 1 and Comparative Example 1 are respectively assembled in an electrolyzer fixture, hydrogen is passed through the cathode side at a flow rate of 50 mL / min, ultrapure water is passed through the anode side at a flow rate of 10 mL / min, a voltage cycle of 0.05-1.23 V is applied on the anode side, and the voltage scan rate is set to 5 mV / s.
[0071] from Figure 4It can be seen that the integrated area surrounded by the green curve of the electrochemical cycle scan corresponding to the catalyst layer prepared by the present invention is significantly higher than the area corresponding to the traditional catalyst layer. Within the voltage cycle CV scan range, the integrated area of the curve is the double electric layer area accessible to the reactants. In other words, the effective electrochemical reaction area in the catalyst layer prepared by the present invention is significantly higher than the effective electrochemical reaction area in the traditional catalyst layer by more than 1.5 times, proving that the present invention greatly improves the catalyst utilization rate in the anode catalyst layer.
[0072] Figure 5 The OER performance test diagram (i.e., electrocatalytic oxygen evolution reaction) of the catalyst layer obtained in Example 1 (i.e., the performance of the agglomerates obtained in the present invention in the figure) and Comparative Example 1 (i.e., the performance of the agglomerates not regulated in the figure) is obtained by linear sweep voltammetry, which can reflect the current response of the catalyst at different voltages. Figure 5 It can be seen that: under high electrolysis voltage, the electrolysis performance of the electrode prepared by the present invention is significantly different from that of the traditional electrode. At the highest electrolysis voltage point tested, the electrolysis current density of the catalyst layer prepared by the present invention is more than 1 times higher than that of the traditional catalyst layer. Under higher electrolysis voltage, the source of the increase in electrolysis current is the reduced transmission loss. This also proves that the loose agglomerate structure prepared by the present invention greatly optimizes the transmission resistance of oxygen inside the agglomerate, thereby achieving the optimization of transmission loss and electrolysis performance.
[0073] The optimized catalyst utilization (indicated by the increased electrochemical effective area) and optimized dissolved oxygen transport resistance (indicated by the increased OER current at high potential) characterized by the RDE technology prove that the aggregate structure regulation achieved by the present invention does enhance the dissolved oxygen transport within the secondary aggregates while liberating more catalyst active sites, thereby improving the catalyst utilization.
[0074] Figure 6 The performance test diagram of membrane electrode water electrolysis obtained by Example 1 (i.e., the membrane electrode performance obtained by the present invention in the figure) and Comparative Example 1 (traditional membrane electrode performance) is as follows: the PEMWE membrane electrodes obtained by Example 1 and Comparative Example 1 are respectively assembled in an electrolytic cell fixture, ultrapure water at a flow rate of 10 mL / min is introduced into the anode side, and 0.01 A / cm is applied to the anode side. 2 ,0.02A / cm 2 ,0.05A / cm 2 ,1A / cm 2 ,2A / cm 2 ,3A / cm 2 ,4A / cm 2 ,5A / cm 2 Current density: each current density is maintained for 600s test time, and the ten-second average potential of the performance stable section is taken as the potential at that current density point.
[0075] from Figure 6 It can be seen that: under high electrolysis current, the difference between the electrolysis voltage of the electrode prepared by the present invention and the traditional electrode is significant. At the highest electrolysis current point tested, the electrolysis voltage of the catalyst layer prepared by the present invention is much lower than that of the traditional catalyst layer. Under higher electrolysis current, the source of the reduction in electrolysis voltage is the reduced concentration polarization loss, which comes from the transmission resistance of oxygen in the anode catalyst layer. This also proves that the loose agglomerate structure prepared by the present invention greatly optimizes the transmission resistance of oxygen inside the agglomerate, thereby achieving the optimization of concentration polarization loss and electrolysis performance.
[0076] The electrolysis current density increased by 2 times, proving the superiority of this scheme in reducing the cost of electrolytic hydrogen production and improving the utilization rate of electrolytic hydrogen production catalysts.
[0077] The electrode membrane electrode obtained in Example 1 and Comparative Example 1 was tested for water electrolysis performance, and the results were as follows:
[0078] Example 1 Comparative Example 1 Transmission overpotential loss <![CDATA[33mV@5A·cm -2 ]]> <![CDATA[330mV@5A·cm -2 ]]> Catalyst utilization <![CDATA[15.48mA·V·cm -2 ]]> <![CDATA[8.44mA·V·cm -2 ]]> active <![CDATA[327.1mA·g -1 @1.6V]]> <![CDATA[200.2mA·g -1 @1.6V]]>
[0079] For the transmission overpotential loss, the overpotential decoupling method is used for calculation. First, the electrolysis current is set to 5A / cm 2 When the high frequency impedance HFR of the anode is measured at this current density, Figure 6 The electrolytic performance iV curve obtained in the experiment is deducted from the ohmic overpotential of the electrolysis voltage at the corresponding current density, that is, V ir-free =V-HFR·iCalculation formula to get iV ir-free For this curve, the electrolysis current density is selected as 0.01A·cm -2 -0.1A·cm -2 The electrolysis current density is calculated by taking the logarithm of the obtained log(i)-V ir-free The curve is linearly fitted to obtain V ir-free =a·log(i)+b. In this case, a is the Tafel slope of the corresponding electrode. act =a·log(i) to obtain the activation overpotential loss at different current densities. At this time, η concentration =V ir-free -η act , the obtained η concentration That is the transmission overpotential loss under the corresponding current density.
[0080] The utilization rate of the catalyst was calculated by the integration method of the CV scanning curve. Figure 4 The absolute area of the curve obtained is directly integrated, and the resulting value is the catalyst utilization rate.
[0081] For the mass activity of the catalyst, Figure 5 The mass activity of the corresponding electrode can be obtained by taking a point from the corresponding LSV performance curve and dividing the electrolysis current density obtained at an electrolysis voltage of 1.6 V by the actual RDE electrode loading.
[0082] Example 2
[0083] The only difference from Example 1 is that the mass concentration of the self-assembly solution A in step (1) is 4%.
[0084] The dispersion solution described in step (4) is a mixture of ultrapure water and isopropanol in a mass ratio of 10:7.
[0085] The mass ratio of the catalyst-ODT self-assembled solid particles C, the perfluorosulfonic acid ionomer solution and the dispersed solution in step (4) is 1.6:1:100.
[0086] The mass ratio of Pt / C catalyst, perfluorosulfonic acid (PFSA) ionomer solution and dispersion solution is 2.5:1:100.
[0087] The rest is the same as in Example 1.
[0088] The electrode membrane electrode prepared in Example 2 was tested for water electrolysis performance using the same testing method as in Example 1. The results are as follows:
[0089] Example 2 Transmission overpotential loss <![CDATA[225mV@5A·cm -2 ]]> Catalyst utilization <![CDATA[10.17mA·V·cm -2 ]]> active <![CDATA[267.53mA·g -1 @1.6V]]>
[0090] It can be seen that the membrane electrode prepared within the scope of the present invention by the method of the present invention has reduced transmission overpotential loss and higher catalyst utilization and activity.
Claims
1. A method for preparing an anode catalyst layer of a proton exchange membrane water electrolysis membrane electrode based on aggregate structure regulation, characterized in that: The method comprises the following steps: (1) mixing n-octadecyl mercaptan and deionized water uniformly to prepare a self-assembly solution A; (2) placing IrOx nanocatalyst particles in self-assembly solution A to obtain catalyst-self-assembly solution B, stirring, ultrasonicating, centrifuging, and washing to obtain solid particles; (3) drying the solid particles obtained in step (2) to obtain catalyst-ODT self-assembled solid particles C; (4) adding the catalyst-ODT self-assembled solid particles C and the perfluorosulfonic acid ionomer solution to the dispersed solution and mixing them to obtain an anode catalyst slurry D; (5) Spray the anode catalyst slurry D onto one side of the proton exchange membrane and dry it to obtain the anode catalyst layer.
2. The preparation method according to claim 1, characterized in that: The mass concentration of the self-assembly solution A described in step (1) is (0.5-4)%.
3. The preparation method according to claim 1, characterized in that: The mass volume ratio of the IrOx nanocatalyst described in step (2) to the self-assembly solution A is (50-100) mg / mL.
4. The preparation method according to claim 1, characterized in that: The drying temperature in step (3) does not exceed 40°C.
5. The preparation method according to claim 1, characterized in that: The dispersion solution described in step (4) is a mixture of ultrapure water and isopropanol in a volume ratio of 10:1-10:
7.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the catalyst-ODT self-assembled solid particles C, the perfluorosulfonic acid ionomer solution and the dispersed solution in step (4) is 1.6:1:500-1.6:1:
100.
7. The preparation method according to claim 1, characterized in that: In step (4), each material is ultrasonically treated in a water bath not exceeding 20° C. for 12-36 hours to obtain an ultrasonically uniform anode catalyst slurry D.
8. An anode catalyst layer of a proton exchange membrane water electrolysis membrane electrode prepared by the preparation method according to any one of claims 1 to 7.
9. An application of the anode catalyst layer of the proton exchange membrane water electrolysis membrane electrode as claimed in claim 8, characterized in that: The anode catalyst layer is applied to a proton exchange membrane water electrolysis membrane electrode.
10. The use of the anode catalyst layer of the proton exchange membrane water electrolysis membrane electrode according to claim 9, characterized in that: The proton exchange membrane water electrolysis membrane electrode is prepared by spraying anode catalyst slurry and cathode catalyst slurry on a proton exchange membrane and on both sides thereof, respectively, and drying them.
Citation Information
Patent Citations
Device and method for inducing bubble coalescence to improve electrolytic efficiency by using microfibers
CN114934278A
Snakelike microchannel electrolysis device suitable for multiphase flow and electrolytic hydrogen production method