A method for preparing UV-resistant cashmere composite fabric
By using the layer-by-layer electrostatic self-assembly technology of nano-chitosan and graphene oxide, graphene oxide is loaded onto the surface of cashmere fabrics, solving the problems of poor washability and high cost of traditional fabrics. This enables the preparation of cashmere composite fabrics with high UV resistance and has broad application prospects.
Patent Information
- Application Number
- CN202211402617.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-10
AI Technical Summary
Traditional UV-blocking fabrics have poor washability, high cost, and are difficult to apply on a large scale. Furthermore, existing methods for preparing UV-resistant textiles are not fast or efficient enough.
Using a layer-by-layer electrostatic self-assembly technique of nano-chitosan (Nano-CS) and graphene oxide (GO), GO is loaded onto the surface of cashmere fabric. By preparing dialdehyde chitosan (D-CS) and nano-chitosan (Nano-CS) solutions, GO is effectively loaded onto cashmere fabric through chemical reaction and charge interaction between Nano-CS and GO.
It enhances the UV resistance of cashmere fabrics, endows them with excellent antibacterial and antistatic properties, and has a simple and efficient preparation method, making it suitable for fields such as smart wearables and UV-resistant fabrics.
Smart Images

Figure CN115852689B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to a method for preparing an anti-ultraviolet cashmere composite fabric. Background Art
[0002] With the intensification of human activities, the ozone layer is constantly being damaged, and more ultraviolet rays can directly irradiate the human body. The impact of excessive ultraviolet radiation on the skin is not only a problem of affecting the beauty of the skin, but also has a serious impact on human health. In order to reduce the harm of ultraviolet rays to the human body, in recent decades, people have continued to deepen their research on anti-ultraviolet textiles. There are two mechanisms of action of anti-ultraviolet textiles: absorption and reflection. Correspondingly, there are two types of ultraviolet shielding agents: absorbers and reflectors (or scatterers). Absorbers and reflectors can be used alone or mixed. Ultraviolet reflectors mainly use the reflection and scattering effects of inorganic particles to prevent ultraviolet rays from penetrating. Ultraviolet absorbers mainly use organic substances to absorb ultraviolet light and convert energy to release or consume energy in the form of heat energy or harmless low radiation. Reflectors are mainly metal oxides such as titanium dioxide, and absorbers are mainly benzophenone compounds, salicylic acid compounds, etc.
[0003] Traditional UV-blocking fabrics are generally manufactured by padding, sol-gel, hydrothermal, etc., which have problems such as poor washability, high cost, and difficulty in large-scale application. The emergence of graphene-based fabrics has solved this problem well. The special two-dimensional structure of graphene not only gives graphene special optical, electrical, magnetic and other properties, but also has excellent anti-ultraviolet, antibacterial, antistatic and other properties. The results show that rGO reduced by graphene oxide (GO) can scatter long-wave ultraviolet rays, absorb high-energy short-wave ultraviolet rays, and convert them into harmless substances such as fluorescence or heat energy. If graphene is loaded on the surface of textile fibers, it will give the textiles good anti-ultraviolet properties. Therefore, compared with traditional methods, the development of a fast, efficient, washable and UV-resistant fabric has a great market prospect. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing an anti-ultraviolet cashmere composite fabric, which can effectively improve the anti-ultraviolet performance of the cashmere fabric, and the preparation method is simple and efficient, so as to solve the problems raised in the above background.
[0005] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:
[0006] The present invention is a method for preparing an ultraviolet-resistant cashmere composite fabric, and the preparation method comprises the following steps:
[0007] S1. preparing a dialdehyde chitosan (D-CS) solution: adding sodium periodate (NaIO4) to a solution of chitosan dissolved in acetic acid under light-proof conditions, terminating with anhydrous ethanol and dialyzing to obtain a D-CS solution;
[0008] S2, prepare nano-chitosan (Nano-CS) solution: dry the D-CS solution obtained in step S1, mix it with acetic acid solution, and then add hydrogen peroxide (H 2 O 2 ) and stirred, then adding Span 80 and sodium tripolyphosphate (TPP) to react to obtain Nano-CS solution;
[0009] S3, preparing cashmere fabric modified with Nano-CS; measuring the Nano-CS solution prepared in step S2, and then immersing the cleaned pure cashmere fabric in the prepared Nano-CS solution, immersing for a period of time, washing and drying, to obtain cashmere fabric modified with Nano-CS;
[0010] S4, preparing cashmere loaded graphene fabric modified by Nano-CS: adding GO powder into deionized water and stirring evenly, obtaining GO solution after ultrasonication, immersing the cashmere fabric modified by Nano-CS in step S43 into the GO solution, and loading GO onto the surface of the cashmere fabric modified by Nano-CS by using the layer-by-layer electrostatic self-assembly technology principle of Nano-CS and GO, and washing and drying after a period of time to obtain the cashmere loaded graphene fabric modified by Nano-CS.
[0011] Preferably, the preparation method comprises the following steps:
[0012] S1. Prepare D-CS solution: add sodium periodate (NaIO4) to a solution of chitosan dissolved in acetic acid under light-proof conditions, and dialyze to obtain a D-CS solution after termination with anhydrous ethanol;
[0013] S2, prepare Nano-CS solution: dry the D-CS solution obtained in step S1, mix it with acetic acid solution, and then add a certain proportion of hydrogen peroxide (H 2 O 2 ) and stirred, then adding Span 80 and sodium tripolyphosphate (TPP) to react to obtain Nano-CS solution;
[0014] S3, preparing different types of Nano-CS solutions: weighing a certain amount of the Nano-CS solution in step S2, putting it into the prepared acetic acid solution and stirring it, preparing Nano-CS solutions with different mass fractions and immersing the Nano-CS solutions for different times;
[0015] S4, preparing cashmere fabric modified with Nano-CS; respectively measuring the Nano-CS solution with different mass fractions and the Nano-CS solution immersed for different times in step S3, and then immersing the cleaned pure cashmere fabric in the prepared Nano-CS solution, and washing and drying after immersion for a period of time to obtain the cashmere fabric modified with Nano-CS;
[0016] S5. Preparation of cashmere-loaded graphene fabric modified with Nano-CS: adding a certain amount of GO powder into deionized water and stirring evenly, obtaining a GO solution after ultrasonic treatment, immersing the cashmere fabric modified with Nano-CS in step S4 into the GO solution, and loading GO onto the surface of the cashmere fabric modified with Nano-CS by using the layer-by-layer electrostatic self-assembly principle of Nano-CS and GO. After a period of time, washing and drying are performed to obtain the cashmere-loaded graphene fabric modified with Nano-CS.
[0017] The present invention has the following beneficial effects:
[0018] 1. The preparation method of the UV-resistant cashmere composite fabric provided by the present invention can effectively load GO on the surface of the cashmere fabric based on the layer-by-layer electrostatic self-assembly technology of Nano-CS and GO, thereby imparting the properties of GO to the cashmere fabric.
[0019] 2. The UV-resistant cashmere composite fabric prepared by this method can not only effectively load GO on the surface of cashmere fabric, but also contain a large number of amino groups (-NH 2 ), carboxyl (-COOH) and other groups can react chemically with the active groups on the surface of GO, further increasing the loading amount of GO on the cashmere fiber, and also effectively improving the UV resistance of the cashmere fabric after loading GO.
[0020] 3. Cashmere has been widely used in daily clothing due to its softness and warmth-keeping properties. The UV-resistant cashmere composite fabric prepared by this method uses GO as an anti-UV finishing agent, and has antibacterial, antistatic and anti-UV properties. It has potential application prospects in the fields of anti-UV fabrics, smart wearables, antibacterial clothing, etc., and has important development significance.
[0021] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0023] Figure 1 The figure is a schematic diagram of the preparation process of UV-resistant cashmere composite fabric;
[0024] Figure 2 The following are scanning electron microscope (SEM) characterization photos of cashmere samples at different magnification ratios;
[0025] Figure 3 The SEM images of cashmere / Nano-CS / GO after configuring different Nano-CS mass fractions;
[0026] Figure 4 XRD spectra of cashmere, GO, cashmere / Nano-CS, and cashmere / Nano-CS / GO;
[0027] Figure 5 XRD spectra of cashmere / Nano-CS / GO modified with different mass fractions of Nano-CS;
[0028] Figure 6 Infrared characterization of cashmere / Nano-CS / GO modified with different mass fractions of Nano-CS;
[0029] Figure 7 The UV resistance characterization of cashmere / Nano-CS / GO modified with different mass fractions of Nano-CS;
[0030] Figure 8 The SEM images of cashmere / Nano-CS / GO after soaking for different times;
[0031] Fig. 9 XRD spectra of cashmere / Nano-CS / GO after soaking for different times;
[0032] Fig.10 Infrared characterization of cashmere / Nano-CS / GO after soaking for different times;
[0033] Fig.11 To characterize the UV resistance of cashmere / Nano-CS / GO after soaking for different times; DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Embodiment 1
[0036] like Figure 1 As shown, the present invention is a method for preparing an anti-ultraviolet cashmere composite fabric, and the preparation method comprises the following steps:
[0037] S1. Take a certain volume of glacial acetic acid and add it to a volumetric flask. Add deionized water to make a 2% acetic acid solution. Dissolve 4g chitosan powder in 200mL 2% acetic acid solution and stir at 60℃ until completely dissolved. Add 4g / L NaIO 4 The mixture was reacted for 2 h in a dark environment, and then 200 mL of anhydrous ethanol was taken to terminate the reaction and dialyzed in a dialysis bag for 48 h. The mixture was then dried at 60° C. to obtain D-CS powder.
[0038] S2, 100 mL of 2% acetic acid and 0.4 g of D-CS were stirred at 70 °C for 30 min, and 3% H 2 O 2 The solution was added to the above solution at a ratio of 1:10. After degradation for 2 to 3 hours, a small amount of Siban 80 was added and reacted for 30 minutes. After the reaction was completed, TPP was added to make its mass fraction 0.2 g / L. After stirring at room temperature for 30 minutes, Nano-CS solution was obtained.
[0039] S3, cutting the cashmere fabric into a shape of 30 cm × 30 cm, washing it in a deionized water solution at room temperature for 2 to 3 hours, and then drying it at 60°C to obtain the washed cashmere fabric. Figure 2 As shown, the cashmere can be seen by scanning electron microscopy (SEM). The surface scales of cashmere are thin, mostly wrapped around the hair shaft in a ring shape, the scales are relatively smooth, and there is no medulla layer. The scales of cashmere fibers tightly wrap around the hair shaft, with very small curling angles, and are relatively smooth and flat, which is consistent with the softer characteristics of cashmere.
[0040] S4. The cleaned cashmere fabric was immersed in Nano-CS solutions with mass fractions of 0.6%, 1.2%, 1.8%, 2.4% and 3%, respectively. After immersion for 2 hours, the fabric was taken out, washed and dried to obtain cashmere fabric modified with Nano-CS.
[0041] S4, placing graphene oxide powder in deionized water, ultrasonicating for 2 hours and stirring for 3 hours to obtain graphene oxide solution. Then, the cashmere fabric modified with Nano-CS is immersed in the GO solution, and after immersion for 2 hours, the cashmere fabric modified with graphene oxide is obtained. Figure 3As shown, scanning electron microscopy (SEM) was used to characterize the five groups of cashmere fabrics modified with Nano-CS, namely 0.6%, 1.2%, 1.8%, 2.4% and 3% from top to bottom. It can be clearly seen that GO is attached to the surface of the fabric in the form of multiple layers of wrinkles. With the increase of the mass fraction of Nano-CS, the loading amount of GO is also significantly improved.
[0042] By preparing dialdehyde chitosan (D-CS) solution and then synthesizing Nano-CS solution, preparing Nano-CS solution with different mass fractions, preparing cashmere fabric modified by Nano-CS, and immersing the cashmere fabric modified by Nano-CS in graphene oxide (GO) solution, GO is loaded onto the surface of cashmere fabric with the help of Nano-CS's "bridge" effect. The anti-ultraviolet performance test results show that its UPF value can reach 500+, and UVA is less than 5%, which has excellent anti-ultraviolet ability, indicating that cashmere fabric with excellent anti-ultraviolet performance can be obtained by surface modification of cashmere fabric with GO and Nano-CS through electrostatic layer-by-layer self-assembly technology, and the modified fabric has good water washing durability of anti-ultraviolet performance. Because graphene materials have excellent electrical, optical, thermal and mechanical properties, they are widely used in the textile field, which opens up new research space for the research and development of functional textiles, and has potential applications in smart wearables, anti-ultraviolet fabrics, anti-static fabrics and other fields.
[0043] Figure 4 The XRD spectra of cashmere, GO, cashmere / Nano-CS and cashmere / Nano-CS / GO are as shown in the figure. In the cashmere / Nano-CS / GO spectrum, the absorption peak shifts. This is because GO reacts with Nano-CS, and the carboxyl groups at the edge of graphene oxide react with the amino groups of nano-chitosan, increasing the interlayer spacing of graphene oxide, so the diffraction angle becomes smaller.
[0044] Figure 5 is the XRD spectrum of cashmere / Nano-CS / GO modified with different mass fractions of Nano-CS. Figure 5 It can be seen that after the cashmere fabric modified with Nano-CS is loaded with GO, the amorphous structure peaks of Nano-CS appear at 2θ of 20.52° and 22.56°; the characteristic peak of GO is at 2θ of 10.48°, which correspond to the corresponding substances respectively.
[0045] Depend on Figure 6It can be seen from the infrared spectrum that in the GO spectrum, 3268cm-1, 1726cm-1, and 1040cm-1 are the stretching vibration peaks of -OH, C=O in -COOH, and CO, respectively. 2921cm-1 is caused by the stretching vibration of -CH3 and -CH2 of cashmere, and the peaks at 1632cm-1 and 1523cm-1 correspond to the carbonyl stretching vibration of secondary amide (amide I band) and the NH bending vibration of amide II band, respectively. In the cashmere / Nano-CS / GO spectrum, it can be seen that the absorption peak at 1523cm-1 is weakened, indicating that the carboxyl group in GO and the amino group in Nano-CS are covalently bonded, and the characteristic stretching vibration band is red-shifted, which may be due to the effect of hydrogen bonds in Nano-CS and GO.
[0046] Figure 7 The anti-ultraviolet effect diagram of cashmere / Nano-CS / GO modified with different mass fractions of Nano-CS is shown in Figure 2. Figure 7 It can be seen that with the increase of Nano-CS mass fraction, the UPF curve shows a trend of first rising and then falling and reaches a maximum at 1.2%, up to 900+, and the overall UVA value is less than 5%, indicating that the composite sample has excellent anti-ultraviolet performance.
[0047] Embodiment 2
[0048] The present invention is a method for preparing an ultraviolet-resistant cashmere composite fabric, and the preparation method comprises the following steps:
[0049] S1. Measure a certain volume of glacial acetic acid and add it to a volumetric flask, make up to volume with deionized water to prepare a 2% volume fraction acetic acid solution, dissolve 4g chitosan powder in 200mL 2% acetic acid solution, stir at 60°C until completely dissolved, add 4g / L NaIO4 to the above solution and react for 2h in the dark, then measure 200mL anhydrous ethanol to terminate the reaction and dialyze in a dialysis bag for 48h, and then dry at 60°C to obtain D-CS powder.
[0050] S2, 100 mL of 2% acetic acid and 0.4 g of D-CS were stirred at 70 °C for 30 min, and 3% H 2 O 2 The solution was added into the above solution at a ratio of 1:10. After degradation for 2-3 hours, a small amount of Siban 80 was added and reacted for 30 minutes. After the reaction was completed, TPP was added to make its mass fraction 0.2 g / L. After stirring at room temperature for 30 minutes, Nano-CS solution was obtained.
[0051] S3. Cut the cashmere fabric into a shape of 30 cm×30 cm, wash it in a deionized water solution at room temperature for 2 to 3 hours, and then dry it at 60° C. to obtain the washed cashmere fabric.
[0052] S4. Immerse the cleaned cashmere fabric in a 0.6% by mass Nano-CS solution, soak for 30 minutes, then take out, wash and dry. Immerse once, three times and five times respectively to obtain three groups of cashmere / Nano-CS fabrics modified with Nano-CS.
[0053] S5. Place graphene oxide powder in deionized water, ultrasonicate for 2 hours and stir for 3 hours to obtain graphene oxide solutions with different mass fractions. Then, dip the cashmere fabric modified with Nano-CS into the GO solution, and take it out after dipping for 2 hours to obtain the graphene oxide cashmere fabric modified with Nano-CS.
[0054] Figure 8 The three groups from top to bottom are cashmere / Nano-CS / GO fabrics after being impregnated once, three times, and five times. Figure 8 It can be seen that with the increase of the number of impregnation times, due to the effect of layer-by-layer self-assembly, the charges of cashmere and Nano-CS are opposite, so GO can be deposited on the surface of cashmere. Therefore, with the increase of the number of impregnation times, the wrinkles formed by the GO sheets on the cashmere surface gradually increase. Fig. 9 Figure 2 is the XRD diffraction spectrum of cashmere / Nano-CS / GO after soaking for different times. It can be seen from the figure that 2θ=11.2° is the characteristic peak of GO, and 2θ=20.95° is the characteristic peak of cashmere. When the cashmere is modified by Nano-CS and then loaded with GO, it is found that the characteristic peak is offset relative to the original characteristic peak of GO, indicating that GO reacts with Nano-CS and the chemical environment changes.
[0055] Fig.10 The infrared characterization diagram of cashmere / Nano-CS / GO after soaking for different times. In the infrared spectrum of GO, 3275cm-1 is the stretching vibration peak of -OH, 1727cm-1 is the stretching vibration peak of C=O, and 1055cm-1 is the stretching vibration peak of CO. 2922cm-1 is caused by the stretching vibration of -CH3 and -CH2 of cashmere, and the peaks at 1639cm-1 and 1517cm-1 correspond to the carbonyl stretching vibration of secondary amide (amide I band) and the NH bending vibration of amide II band, respectively. In the cashmere / Nano-CS / GO spectrum, it can be seen that the absorption peak at 1517cm-1 is weakened, indicating that the carboxyl group in GO and the amino group in Nano-CS are covalently bound and the two react.
[0056] Fig.11This is the anti-ultraviolet effect diagram of cashmere / Nano-CS / GO fabric after being immersed in Nano-CS solution for different times. It can be seen from the figure that with the increase of the number of immersion in Nano-CS solution, the UPF value of the composite fabric gradually increases, and can reach up to 160+, and the minimum UVA can reach 0.5%, which is lower than 5%, meeting the anti-ultraviolet standard of textiles.
[0057] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0058] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing an anti-ultraviolet cashmere composite fabric, characterized in that: The preparation method comprises the following steps: S1. Prepare D-CS solution: add sodium periodate (NaIO4) to a solution of chitosan dissolved in acetic acid under light-proof conditions, and dialyze to obtain a D-CS solution after termination with anhydrous ethanol; S2, preparing Nano-CS solution: drying the D-CS solution obtained in step S1, mixing it with acetic acid solution, adding a certain proportion of hydrogen peroxide (H2O2) and stirring, and then adding Span 80 and sodium tripolyphosphate (TPP) to react to obtain Nano-CS solution; S3, preparing different types of Nano-CS solutions: weighing a certain amount of the Nano-CS solution in step S2, putting it into the prepared acetic acid solution and stirring it, preparing Nano-CS solutions with different mass fractions and immersing the Nano-CS solutions for different times; S4, preparing cashmere fabric modified with Nano-CS; respectively measuring the Nano-CS solution with different mass fractions and the Nano-CS solution immersed for different times in step S3, and then immersing the cleaned pure cashmere fabric in the prepared Nano-CS solution, and washing and drying after immersion for a period of time to obtain the cashmere fabric modified with Nano-CS; S5. Preparation of cashmere-loaded graphene fabric modified with Nano-CS: adding a certain amount of GO powder into deionized water and stirring evenly, obtaining a GO solution after ultrasonic treatment, immersing the cashmere fabric modified with Nano-CS in step S4 into the GO solution, and loading GO onto the surface of the cashmere fabric modified with Nano-CS by using the layer-by-layer electrostatic self-assembly technology principle of Nano-CS and GO, and washing and drying after a period of time to obtain the cashmere-loaded graphene fabric modified with Nano-CS.
Citation Information
Patent Citations
Self-assembled nanosphere and preparation method and application method thereof
AU2020102161A4
Preparation method of anti-ultraviolet cotton fabric with electrical conductivity
CN110093775A
Method for preparing antibacterial fabric through layer-by-layer self-assembly
CN112680964A
Method for constructing surface of fabric with ultraviolet protection and wash-resistant special wetting functions
WO2016115980A1