Flame retardant wool fabric and preparation method thereof

Polyphosphoric acid containing double bonds and octaamino-POSS are prepared through polymerization reaction to form a modified liquid for chemically modifying wool fabrics, which solves the problem of insufficient flame retardant performance of wool fabrics in the existing technology and achieves efficient and durable Flame retardant effect and low cost production.

CN115852697BActive Publication Date: 2024-10-29TIANJIN YUFENGMA INFORMATION TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211550157.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-10-29
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

Existing wool fabrics have insufficient flame retardant properties, especially in terms of washing resistance and cost, making it difficult to meet strict usage requirements.

Method used

Through the reaction of polyphosphoric acid and acryloyl chloride, and the reaction of octaamino-POSS and acryloyl chloride, polyphosphoric acid and octaamino-POSS containing double bonds are prepared, and polymerized with acrylic acid and sodium methacrylate sulfonate to form a modified Sexual liquid, used to chemically modify wool fabrics to improve their flame retardant properties.

Benefits of technology

The limiting oxygen index of the wool fabric has reached more than 29%. It has excellent flame retardant properties and its performance is not weakened after multiple washings. The process is simple and low-cost, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003980670800000041
    Figure BDA0003980670800000041
  • Figure BDA0003980670800000071
    Figure BDA0003980670800000071
Patent Text Reader

Abstract

The present invention relates to a flame-retardant wool fabric and a preparation method thereof, characterized in that the fabric can be prepared by the following method: first, polyphosphoric acid is reacted with acryloyl chloride to obtain polyphosphoric acid containing double bonds; octaamino-POSS is reacted with acryloyl chloride to obtain octaamino-POSS containing double bonds; then, polyphosphoric acid containing double bonds, octaamino-POSS containing double bonds, acrylic acid and sodium methacrylic acid are polymerized to obtain a modified liquid; the wool fabric is chemically modified in the modified liquid to obtain a flame-retardant wool fabric. The initial limiting oxygen index of the flame-retardant wool fabric prepared by the present invention reaches more than 29%, which belongs to the range of flame-retardant materials; after 5 times of water washing, its limiting oxygen index does not decrease significantly, and still reaches more than 28%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabric preparation, and particularly relates to a flame retardant wool fabric and a preparation method thereof. Background Art

[0002] With the progress of society, the consumption of various civil and industrial textiles has increased rapidly, especially the demand for various indoor and cabin covering fabrics such as curtains, draperies, wall coverings, carpets, furniture fabrics and bedding (pajamas, bedspreads, sheets, quilts, etc.). But at the same time, fires caused by textiles are also increasing, causing huge losses. Therefore, giving textiles flame retardant properties is of great practical significance to ensure safety, reduce the number of fires and the losses caused by them.

[0003] Wool fabric is made of wool fiber as raw material. Wool fiber is an important raw material in the textile industry, with excellent properties such as good moisture absorption, warmth and comfort, and soft feel. Moreover, as a natural fiber containing keratin, wool fiber has certain flame retardancy compared with other fibers. This is because wool has high nitrogen content (16%), high ignition point (>500℃), low combustion heat, and high moisture regain (10%~14%).

[0004] Although wool fiber has certain flame retardant properties, it still cannot meet the more stringent use occasions. With the increase in demand for various wool textiles and the improvement of flame retardant requirements, more and more attention has been paid to the flame retardant research of wool fabrics.

[0005] Literature research shows that the flame retardant properties of wool fabrics have received widespread attention. At present, the preparation method of flame retardant wool fabrics is mainly to immerse the wool fabric in a prepared flame retardant solution to make the fabric have high flame retardant properties; for example: Chinese invention patent application No. 201811037875.3 discloses a method for preparing flame retardant wool fabrics: immersing the wool fabric in the prepared phosphorus-containing silica sol, squeezing the liquid to a liquid rate of 90-100%, and then drying, drying, washing, and airing to obtain flame retardant wool fabrics; Chinese invention patent application No. 201210200002.6 discloses a method for flame retardant treatment of wool fibers: using nitric acid-modified carbon balls as flame retardants, deionized water, γ-mercaptopropyltriethoxysilane to prepare a carbon ball flame retardant suspension, immersing the wool fiber in the carbon ball flame retardant suspension, heating to 70°C in a microwave reactor for microwave irradiation, and then flame retardant treatment in an ultrasonic disperser. However, the flame-retardant wool fabrics prepared by the above methods still have many shortcomings, such as: the first method uses phosphorus-containing silica sol to flame-retardant wool fibers, but its washing resistance deteriorates and cannot achieve a permanent flame-retardant effect; the second method has cumbersome steps, high flame-retardant costs, and is not suitable for large-scale production. Therefore, it is necessary to improve the flame-retardant process of wool fabrics in the prior art to obtain wool fabrics with excellent flame-retardant properties. Summary of the invention

[0006] In view of the above-mentioned drawbacks existing in the prior art, the object of the present invention is to provide a flame retardant wool fabric and a preparation method thereof.

[0007] The invention aims to provide a flame-retardant wool fabric, which can be prepared by the following method: first, polyphosphoric acid is reacted with acryloyl chloride to obtain polyphosphoric acid containing double bonds; octaamino-POSS is reacted with acryloyl chloride to obtain octaamino-POSS containing double bonds; then, the polyphosphoric acid containing double bonds, octaamino-POSS containing double bonds, acrylic acid and sodium methyl propylene sulfonate are polymerized to obtain a modified liquid; and the wool fabric is chemically modified in the modified liquid to obtain the flame-retardant wool fabric.

[0008] Another object of the present invention is to provide a method for preparing a flame retardant wool fabric, the specific method comprising the following steps:

[0009] (1) Reaction of polyphosphoric acid and acryloyl chloride: Under ice bath conditions, 3-5 g of acryloyl chloride is added to a three-necked flask containing 50-100 mL of tetrahydrofuran, and stirred to dissolve to obtain a tetrahydrofuran solution containing acryloyl chloride; 5-10 g of polyphosphoric acid and 2-4 g of potassium carbonate are dissolved in 100-200 mL of tetrahydrofuran to obtain a mixed solution, and then the mixed solution is added dropwise to the tetrahydrofuran solution containing acryloyl chloride; after the addition is completed, the reaction is continued with stirring for a period of time, the tetrahydrofuran solvent in the reaction solution is evaporated and removed, the reaction product is washed with ethanol, and finally the product is dried to obtain a polyphosphoric acid containing double bonds.

[0010] Preferably, the dripping time is 1 to 3 hours, and the stirring reaction time after the dripping is completed is 2 to 3 hours.

[0011] Preferably, the drying conditions are: vacuum drying, drying time 10 to 20 hours, and drying temperature 30 to 50°C.

[0012] (2) Reaction of octaamino-POSS and acryloyl chloride: 5-7 g of octaamino-POSS and 1-2 g of triethylamine were dissolved in 150 mL of tetrahydrofuran in a four-necked flask under ice bath conditions. The mixture was stirred under ice bath conditions and N 2 Protection, 4-6g acryloyl chloride is dissolved in 100mL tetrahydrofuran, and tetrahydrofuran containing octaamino-POSS and triethylamine is added dropwise to the tetrahydrofuran containing acryloyl chloride at a dropping speed of 1-3 drops / second. After the addition is completed, the reaction is carried out in an ice bath at a constant temperature. After the reaction is completed, the reaction is filtered under reduced pressure, rotary evaporated, and dried to obtain octaamino-POSS containing a double bond.

[0013] Preferably, the reaction time is 10 to 14 hours.

[0014] (3) Preparation of modified liquid: In 200 mL of tap water, add the double-bond-containing polyphosphoric acid obtained in step (1), the double-bond-containing octaamino-POSS obtained in step (2), acrylic acid and sodium methyl propylene sulfonate, and stir and dissolve them at 50-60° C. to obtain a mixed solution; dissolve ammonium persulfate in 50 mL of tap water, and add the tap water containing ammonium persulfate dropwise to the mixed solution under stirring for 30-60 minutes. After the dropwise addition is completed, keep the mixture warm for 2-4 hours to obtain a modified liquid.

[0015] Preferably, the usage ratio of the double-bond-containing polyphosphoric acid (g) prepared in step (1), the double-bond-containing octaamino-POSS (g) prepared in step (2), acrylic acid (mL), sodium methyl methacrylate sulfonate (g) and ammonium persulfate (g) is: 1:1-2:4-6:1-2:0.1-0.2.

[0016] (4) Preparation of flame-retardant wool fabric: dilute the modified liquid obtained in step (3) with tap water by 5 to 7 times to obtain a dilution, add sodium chloride to the dilution, adjust the pH of the dilution to 5 to 6 with 10% hydrochloric acid, immerse the wool fabric in the dilution at 80 to 90° C. for 30 to 60 minutes, rinse with tap water 3 to 5 times after immersion, and dry to obtain a flame-retardant wool fabric.

[0017] Preferably, the usage ratio of the sodium chloride (g) to the diluent (mL) is 1:100-120; the usage ratio of the wool fabric (g) to the diluent (mL) is 1:30-50.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present invention realizes the grafting of organic silicon- and phosphorus-containing polymers onto the surface of wool fabrics, and this method significantly improves the flame retardant properties of wool fabrics.

[0020] (2) The inventors of the present application unexpectedly discovered that the initial limiting oxygen index of the flame-retardant wool fabric prepared by the present invention reached more than 29%, which is within the range of flame-retardant materials; after five times of washing, its limiting oxygen index did not decrease significantly and still reached more than 28%.

[0021] (3) The present invention obtains organic silicon and phosphorus-containing polymers prepared by polymerization reaction. Organic silicon and phosphorus-containing polymers are excellent flame retardants. Therefore, the prepared wool fabric also has excellent flame retardant properties.

[0022] (4) The inventors of the present application unexpectedly discovered that by chemically reacting silicone and phosphorus-containing polymers with wool fabric, a strong bond between the two can be achieved; further discovered that the flame retardant properties of the wool fabric remain unchanged after multiple washings.

[0023] (5) The flame-retardant wool fabric prepared by the method of the present invention has strong flame retardancy, the entire production process is simple, the price is low, and the production process has little pollution to the environment. DETAILED DESCRIPTION

[0024] The following examples and comparative examples illustrate the present invention in detail.

[0025] Sources of main raw materials: The flame-retardant wool fabrics were purchased from Xinxiang Zhuocheng Special Textile Co., Ltd. Octaamino-POSS was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., and its molecular structure is as follows:

[0026]

[0027] Example 1

[0028] A method for preparing a flame-retardant wool fabric in this embodiment comprises the following steps:

[0029] (1) Reaction of polyphosphoric acid and acryloyl chloride: 4 g of acryloyl chloride was added to a three-necked flask containing 75 mL of tetrahydrofuran under ice bath conditions, and the mixture was stirred to dissolve to obtain a tetrahydrofuran solution containing acryloyl chloride; 7.5 g of polyphosphoric acid and 3 g of potassium carbonate were dissolved in 150 mL of tetrahydrofuran to obtain a mixed solution, and then the mixed solution was added dropwise to the tetrahydrofuran solution containing acryloyl chloride; the dropping time was 2 h, and the stirring reaction time was continued for 2.5 h after the dropping was completed, the tetrahydrofuran solvent in the reaction solution was evaporated and removed, the reaction product was washed with ethanol, and finally the product was dried under the conditions of vacuum drying, drying time of 15 h, and drying temperature of 40° C. to obtain polyphosphoric acid containing double bonds.

[0030] (2) Reaction of octaamino-POSS with acryloyl chloride: 6 g of octaamino-POSS and 1.5 g of triethylamine were dissolved in 150 mL of tetrahydrofuran in a four-necked flask under ice bath conditions. The mixture was stirred under ice bath conditions and N 2 Protection, 5g of acryloyl chloride was dissolved in 100mL of tetrahydrofuran, and tetrahydrofuran containing octaamino-POSS and triethylamine was added dropwise to the tetrahydrofuran containing acryloyl chloride at a rate of 2 drops / second. After the addition was completed, the reaction was carried out in an ice bath at a constant temperature for 12h. After the reaction was completed, the reaction was filtered under reduced pressure, rotary evaporated, and dried to obtain octaamino-POSS containing a double bond.

[0031] (3) Preparation of modified liquid: In 200 mL of tap water, add 1 g of the double-bond polyphosphoric acid obtained in step (1), 1.5 g of the double-bond octaamino-POSS obtained in step (2), 5 mL of acrylic acid and 1.5 g of sodium methyl propylene sulfonate, and stir and dissolve them at 55° C. to obtain a mixed solution; dissolve 0.15 g of ammonium persulfate in 50 mL of tap water, and add the tap water containing ammonium persulfate dropwise to the mixed solution under stirring for 45 minutes. After the addition is completed, keep the mixture warm for 3 hours to obtain a modified liquid.

[0032] (4) Preparation of flame-retardant wool fabric: The modified liquid obtained in step (3) was diluted 6 times with tap water to obtain a diluent, sodium chloride was added to the diluent, and the pH of the diluent was adjusted to 5.5 with 10% hydrochloric acid. The wool fabric was immersed in the diluent at 85°C for 45 minutes. After the immersion, the fabric was rinsed with tap water for 4 times and dried to obtain a flame-retardant wool fabric. The ratio of sodium chloride (g) to the diluent (mL) was 1:110; the ratio of wool fabric (g) to the diluent (mL) was 1:40.

[0033] Example 2

[0034] A method for preparing a flame-retardant wool fabric in this embodiment comprises the following steps:

[0035] (1) Reaction of polyphosphoric acid and acryloyl chloride: 3 g of acryloyl chloride was added to a three-necked flask containing 50 mL of tetrahydrofuran under ice bath conditions, and the mixture was stirred to dissolve to obtain a tetrahydrofuran solution containing acryloyl chloride; 5 g of polyphosphoric acid and 2 g of potassium carbonate were dissolved in 100 mL of tetrahydrofuran to obtain a mixed solution, and then the mixed solution was added dropwise to the tetrahydrofuran solution containing acryloyl chloride; the dropping time was 2 h, and the stirring reaction time was continued for 2.5 h after the dropping was completed. The tetrahydrofuran solvent in the reaction solution was evaporated and removed, and the reaction product was washed with ethanol. Finally, the product was dried under the following drying conditions: vacuum drying, drying time 10 h, and drying temperature 30° C. to obtain polyphosphoric acid containing double bonds.

[0036] (2) Reaction of octaamino-POSS with acryloyl chloride: 5 g of octaamino-POSS and 1 g of triethylamine were dissolved in 150 mL of tetrahydrofuran in a four-necked flask under ice bath conditions. The mixture was stirred under ice bath conditions and N 2 Protection, 4g of acryloyl chloride was dissolved in 100mL of tetrahydrofuran, and tetrahydrofuran containing octaamino-POSS and triethylamine was added dropwise to the tetrahydrofuran containing acryloyl chloride at a dropping speed of 1 drop / second. After the addition was completed, the reaction was carried out in an ice bath at a constant temperature for 10 hours. After the reaction was completed, the reaction was filtered under reduced pressure, rotary evaporated, and dried to obtain octaamino-POSS containing a double bond.

[0037] (3) Preparation of modified liquid: In 200 mL of tap water, add 1 g of the double-bond polyphosphoric acid obtained in step (1), 1 g of the double-bond octaamino-POSS obtained in step (2), 4 mL of acrylic acid and 1 g of sodium methyl propylene sulfonate, and stir and dissolve them at 50° C. to obtain a mixed solution; dissolve 0.1 g of ammonium persulfate in 50 mL of tap water, and add the tap water containing ammonium persulfate dropwise to the mixed solution under stirring for 30 minutes. After the addition is completed, keep the mixture warm for 2 hours to obtain a modified liquid.

[0038] (4) Preparation of flame-retardant wool fabric: The modified liquid obtained in step (3) is diluted 6 times with tap water to obtain a diluent, sodium chloride is added to the diluent, and the pH of the diluent is adjusted to 5.0 with 10% hydrochloric acid. The wool fabric is immersed in the diluent at 85° C. for 30 minutes. After the immersion, the fabric is rinsed with tap water for 3 times and dried to obtain a flame-retardant wool fabric. The ratio of sodium chloride (g) to the diluent (mL) is 1:100; the ratio of wool fabric (g) to the diluent (mL) is 1:30.

[0039] Example 3

[0040] A method for preparing a flame-retardant wool fabric in this embodiment comprises the following steps:

[0041] (1) Reaction of polyphosphoric acid and acryloyl chloride: Under ice bath conditions, 5 g of acryloyl chloride was added to a three-necked flask containing 100 mL of tetrahydrofuran, and stirred to dissolve to obtain a tetrahydrofuran solution containing acryloyl chloride; 10 g of polyphosphoric acid and 4 g of potassium carbonate were dissolved in 200 mL of tetrahydrofuran to obtain a mixed solution, and then the mixed solution was added dropwise to the tetrahydrofuran solution containing acryloyl chloride; the dropping time was 3 h, and the stirring reaction time was continued for 3 h after the dropping was completed, the tetrahydrofuran solvent in the reaction solution was evaporated and removed, and the reaction product was washed with ethanol. The drying conditions were: vacuum drying, drying time 20 h, drying temperature 50°C, and finally the product was dried to obtain polyphosphoric acid containing double bonds.

[0042] (2) Reaction of octaamino-POSS with acryloyl chloride: 7 g of octaamino-POSS and 2 g of triethylamine were dissolved in 150 mL of tetrahydrofuran in a four-necked flask under ice bath conditions. The mixture was stirred under ice bath conditions and N 2 Protection, 6g of acryloyl chloride was dissolved in 100mL of tetrahydrofuran, and tetrahydrofuran containing octaamino-POSS and triethylamine was added dropwise to the tetrahydrofuran containing acryloyl chloride at a rate of 3 drops / second. After the addition was completed, the reaction was carried out in an ice bath at a constant temperature for 14h. After the reaction was completed, the reaction was filtered under reduced pressure, rotary evaporated, and dried to obtain octaamino-POSS containing a double bond.

[0043] (3) Preparation of modified liquid: In 200 mL of tap water, add 1 g of the double-bond polyphosphoric acid obtained in step (1), 2 g of the double-bond octaamino-POSS obtained in step (2), 6 mL of acrylic acid and 2 g of sodium methyl propylene sulfonate, and stir and dissolve them at 50-60° C. to obtain a mixed solution; dissolve 0.2 g of ammonium persulfate in 50 mL of tap water, and add the tap water containing ammonium persulfate dropwise to the mixed solution under stirring for 60 minutes. After the addition is completed, keep the mixture warm for 4 hours to obtain a modified liquid.

[0044] (4) Preparation of flame-retardant wool fabric: The modified liquid obtained in step (3) is diluted 7 times with tap water to obtain a diluent, sodium chloride is added to the diluent, and the pH of the diluent is adjusted to 6 with 10% hydrochloric acid. The wool fabric is immersed in the diluent at 90° C. for 60 minutes. After the immersion, the fabric is rinsed with tap water 5 times and dried to obtain a flame-retardant wool fabric. The ratio of sodium chloride (g) to the diluent (mL) is 1:120; the ratio of wool fabric (g) to the diluent (mL) is 1:50.

[0045] Comparative Example A

[0046] Taking Example 1 as a comparison, in this comparative example, the "4 g acryloyl chloride" in step (1) is reduced to "0.4 g acryloyl chloride", and the other preparation methods are implemented according to the preparation method of Example 1.

[0047] Comparative Example B

[0048] Taking Example 1 as a comparison, in this comparative example, the "4 g acryloyl chloride" in step (1) is increased to "20 g acryloyl chloride", and the other preparation methods are implemented according to the preparation method of Example 1.

[0049] Comparative Example C

[0050] Taking Example 1 as a comparison, in this comparative example, in step (2), "6 g of octaamino-POSS" is reduced to "0.6 g of octaamino-POSS", and the other preparation methods are implemented according to the preparation method of Example 1.

[0051] Comparative Example D

[0052] Taking Example 1 as a comparison, in this comparative example, in step (2), "6 g of octaamino-POSS" is increased to "30 g of octaamino-POSS", and the other preparation methods are implemented according to the preparation method of Example 1.

[0053] Comparative Example E

[0054] Taking Example 1 as a comparison, in this comparative example, in step (4), "the usage ratio of the wool fabric (g) to the diluent (mL) is: 1:40" is changed to "the usage ratio of the wool fabric (g) to the diluent (mL) is: 1:4", and the other preparation methods are implemented according to the preparation method of Example 1.

[0055] Comparative Example F

[0056] Taking Example 1 as a comparison, in this comparative example, in step (4), "the usage ratio of the wool fabric (g) to the diluent (mL) is: 1:40" is changed to "the usage ratio of the wool fabric (g) to the diluent (mL) is: 1:400", and the other preparation methods are implemented according to the preparation method of Example 1.

[0057] Performance evaluation example:

[0058] In order to better detect the flame retardancy of the wool fabric prepared in the present invention, the flame retardancy of the wool fabric prepared in the above specific examples 1 to 3 and comparative examples A to F of the present invention and the purchased flame retardant wool fabric were tested. The test method adopted the oxygen index test method, that is, according to GB / T5454-1997 "Textile Combustion Performance Test Oxygen Index Method", the wool fabric was subjected to standard washing with reference to the washing method of the washing fastness tester of GB / T20944.1-2007. The test results are shown in Table 1.

[0059] Table 1 Flame retardant test results of wool fabrics prepared in Examples 1 to 3 and Comparative Examples A to F and purchased wool fabrics before washing and after washing for 5 times

[0060]

[0061] The limiting oxygen index LOI is one of the important indicators of flame retardant materials. Generally, materials with a limiting oxygen index greater than 28% are flame retardant materials. As can be seen from Table 1, the initial limiting oxygen index of the flame retardant wool fabric prepared by the present invention reaches more than 29%, which belongs to the range of flame retardant materials; after 5 times of water washing, its limiting oxygen index does not decrease significantly, and still reaches more than 28%. After 5 times of water washing, the flame retardant performance of the flame retardant wool fabric prepared by the present invention is slightly higher than the flame retardant performance of the purchased flame retardant wool fabric. In addition, the limiting oxygen index of the wool fabric prepared by comparative example AF is small, which shows that the amount of acryloyl chloride, the amount of octaamino-POSS, and the ratio of fabric to diluent all have an important influence on the flame retardant performance of the wool fabric. The flame retardant performance experimental test shows that the flame retardant wool fabric prepared by the present invention has a good flame retardant effect and is a qualified flame retardant wool fabric.

Claims

1. A method for preparing flame retardant wool fabric, It is characterized in that The preparation method is as follows: The modified liquid is diluted 5 to 7 times with tap water to obtain a dilution solution, sodium chloride is added to the dilution solution, the pH value of the dilution solution is adjusted to 5 to 6 with 10% hydrochloric acid, the wool fabric is immersed in the dilution solution at 80 to 90° C. for 30 to 60 minutes, and after the immersion, the wool fabric is rinsed with tap water for 3 to 5 times and dried to obtain a flame-retardant wool fabric; wherein the initial limiting oxygen index of the flame-retardant wool fabric is higher than 29%, and after 5 times of water washing, the limiting oxygen index is higher than 28%; The preparation method of the modified liquid is as follows: adding polyphosphoric acid containing double bonds, octaamino-POSS containing double bonds, acrylic acid and sodium methyl propylene sulfonate to 200 mL of tap water, stirring and dissolving at 50-60° C. to obtain a mixed solution; dissolving ammonium persulfate in 50 mL of tap water, and dripping the tap water containing ammonium persulfate into the mixed solution under stirring conditions for 30-60 minutes. After the dripping is completed, heat-retaining and reacting for 2-4 hours to obtain the modified liquid; The dosage ratio of the double-bond-containing polyphosphoric acid, double-bond-containing octaamino-POSS, acrylic acid, sodium methyl propylene sulfonate and ammonium persulfate is: 1g: (1-2)g: (4-6)mL: (1-2)g: (0.1-0.2)g.

2. A method for preparing a flame retardant wool fabric according to claim 1, It is characterized in that The dosage ratio of the sodium chloride to the diluent is 1 g: (100-120) mL; the dosage ratio of the wool fabric to the diluent is 1 g: (30-50) mL.

3. The method for preparing a flame retardant wool fabric according to claim 1, It is characterized in that The preparation method of the double-bond-containing octaamino-POSS is as follows: 5-7 g of octaamino-POSS and 1-2 g of triethylamine are dissolved in 150 mL of tetrahydrofuran in a four-necked flask under ice bath conditions, and the mixture is stirred in an ice bath and passed through N 2 Protection, 4-6g acryloyl chloride is dissolved in 100mL tetrahydrofuran, and tetrahydrofuran containing octaamino-POSS and triethylamine is added dropwise to the tetrahydrofuran containing acryloyl chloride at a dropping speed of 1-3 drops / second. After the addition is completed, the reaction is carried out in an ice bath at a constant temperature. After the reaction is completed, the reaction is filtered under reduced pressure, rotary evaporated, and dried to obtain octaamino-POSS containing a double bond.

4. A method for preparing a flame retardant wool fabric according to claim 3, It is characterized in that The reaction time is 10 to 14 hours.

5. The method for preparing a flame retardant wool fabric according to claim 1, It is characterized in that The preparation method of the double-bond-containing polyphosphoric acid comprises the following steps: adding 3-5 g of acryloyl chloride into a three-necked flask containing 50-100 mL of tetrahydrofuran under ice bath conditions, stirring and dissolving to obtain a tetrahydrofuran solution containing acryloyl chloride; dissolving 5-10 g of polyphosphoric acid and 2-4 g of potassium carbonate in 100-200 mL of tetrahydrofuran to obtain a mixed solution, and then dripping the mixed solution into the tetrahydrofuran solution containing acryloyl chloride; after the dripping is completed, stirring and reacting for a period of time, evaporating and removing the tetrahydrofuran solvent in the reaction solution, washing the reaction product with ethanol, and finally drying the product to obtain the double-bond-containing polyphosphoric acid.

6. A method for preparing a flame retardant wool fabric according to claim 5, It is characterized in that The time of the dropwise addition is 1 to 3 hours, and the time of continuing the stirring reaction after the dropwise addition is 2 to 3 hours.

7. The method for preparing a flame retardant wool fabric according to claim 5, It is characterized in that The drying conditions are: vacuum drying, drying time 10 to 20 hours, and drying temperature 30 to 50°C.

8. A flame retardant wool fabric, It is characterized in that The flame retardant wool fabric is prepared by the method for preparing the flame retardant wool fabric according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Flame-retardant treatment method for wool fibers

    CN102720053A

  • Preparation method of flame retardant wool fabric

    CN109252357A

  • Preparation method and application of epoxy-based POSS (polyhedral oligomeric silsesquioxane) / ammonium polyphosphate composite flame retardant

    CN107190515A

  • Flame-retardant composition

    JP2003292793A