A kind of reactive polyurethane hot melt adhesive and preparation method thereof
By using crystalline polyester polyol, hydroxyl polyolefin polymer and other components in reactive polyurethane hot melt adhesive, the problem of insufficient bonding strength and hydrolysis resistance to weakly polar plastic substrates is solved, and the problem of weakly polar plastic substrates is realized. Efficient bonding of polar substrates and improvement of high temperature and humidity resistance.
Patent Information
- Application Number
- CN202211510565.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-29
AI Technical Summary
Existing reactive polyurethane hot melt adhesives have insufficient bonding strength to weakly polar plastic substrates and low hydrolysis resistance, which cannot meet the needs of modern industry for high dielectric strength and reliable performance.
It uses components such as crystalline polyester polyol, hydroxyl polyolefin polymer, hydroxyl-terminated liquid nitrile rubber, thermoplastic resin, isocyanate and coupling agent to form a reactive polyurethane hot melt adhesive through a specific preparation method to improve the resistance to weak poles. Adhesion and hydrolysis resistance of the base material.
Significantly improves the bonding strength, thermal stability, hydrolysis resistance and electrical properties of the reactive polyurethane hot melt adhesive to weakly polar substrates, prolongs the use time of the product, and maintains high performance under high temperature and high humidity conditions. Bonding strength and dielectric strength.
Smart Images

Figure CN115873548B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a reactive polyurethane hot melt adhesive and a preparation method thereof, belonging to the technical field of adhesives. Background Art
[0002] Hot melt adhesives usually refer to adhesives that are solid at room temperature, melt into liquid form when heated, and complete bonding within a few seconds after being applied and wetted to the adherends, pressed and cooled.
[0003] Ordinary polyurethane hot melt adhesive can flow after heating and can be easily applied to the adherend. Once cooled, it immediately solidifies to produce cohesion, so that the two adherends are bonded. It is very popular in the modern automated assembly industry for its low pollution, high initial viscosity and fast adhesion, and has developed rapidly. However, due to the thermoplasticity of its main resin, it is easy to creep when heated and become brittle when cooled, thus affecting the mechanical strength and performance; and its high melting temperature makes it unsuitable for heat-sensitive adherends, so its application in modern industry is subject to certain restrictions.
[0004] Reactive polyurethane hot melt adhesive is a polyurethane system that introduces reactive active groups. After heating and coating, it is cooled and solidified to produce cohesion, so that the two adherends are bonded to produce bonding force. Then, through the reaction of the active groups, it is further cross-linked and solidified to form a thermosetting resin; thereby improving the bonding strength and having properties such as heat resistance, solvent resistance, drug resistance, and creep resistance. Therefore, in addition to the characteristics of ordinary hot melt adhesives, reactive polyurethane hot melt adhesives are also reactive.
[0005] Most reactive polyurethane hot melt adhesives have high bonding strength and obvious advantages to most metal and polar plastic substrates due to their raw materials, especially the strong polarity of isocyanate groups. However, at the same time, they have poor bonding to weak polar materials, such as PS, ABS and other materials. Before using reactive polyurethane hot melt adhesives, such substrates must be pre-treated by primer, plasma treatment and other pretreatments, which adds additional processes and costs. However, with the needs of market development, some components are widely used in order to meet the requirements of lightweight and electrical performance, especially in the field of 5G communications. High dielectric constant strength modified plastics are ready to go. In order to meet the requirements of high dielectric strength, weak polarity high dielectric strength plastic components are used. Wearable devices such as VR and AR also have such requirements. Therefore, the corresponding reactive polyurethane hot melt adhesives not only require further requirements for various substrates, including bonding strength and other properties of weak polar plastics, but also need to improve their dielectric strength. In addition, the reliability of various components also needs to be improved, especially hydrolysis resistance. However, the current reactive polyurethane hot melt adhesive has a relatively strong selectivity for the adhesion of substrates, especially for weakly polar plastic substrates, the bonding strength does not meet customer needs, and the dielectric strength is low. Due to the presence of a large number of strongly polar functional groups such as ester bonds, hydrolysis will occur under long-term moisture, resulting in reduced adhesion performance or even failure. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a reactive polyurethane hot melt adhesive and a preparation method thereof, which is suitable for bonding various substrates, especially having excellent bonding performance to weakly polar substrates and good hydrolysis resistance.
[0007] The technical solution of the present invention to solve the above technical problems is as follows:
[0008] A reactive polyurethane hot melt adhesive comprises the following components in parts by weight:
[0009] 25-30 parts of crystalline polyester polyol, 15-20 parts of hydroxyl polyolefin polymer, 15-20 parts of hydroxyl-terminated liquid nitrile rubber, 15-20 parts of thermoplastic resin, 20-30 parts of isocyanate, 0.5-1.0 parts of coupling agent, and 0.1-0.5 parts of catalyst.
[0010] On the basis of the above technical solution, the present invention can also make the following improvements:
[0011] Furthermore, the crystalline polyester polyol is 1,6-hexanediol adipate (HDO / AA).
[0012] The beneficial effect of adopting the above further technical solution is that the presence of the crystalline polyester improves the initial bonding strength and the final strength of the system and shortens the open time of the product.
[0013] Further, the hydroxyl polyolefin polymer has the following structure:
[0014]
[0015] , where the value range of X is 10-22 and the value range of Y is 2-14.
[0016] The beneficial effect of adopting the above further technical solution is that the presence of hydroxyl groups enables the polyolefin structure to react into the entire molecular structure. The presence of the polyolefin structure improves the bonding strength of the system to weakly polar substrates, and improves the thermal stability, hydrolysis resistance and electrical properties of the system.
[0017] Furthermore, the hydroxyl value of the hydroxyl-terminated liquid nitrile rubber is in the range of 20-60 mgKOH / g, and the nitrile content is 24±2%.
[0018] The beneficial effects of adopting the above further technical solution are: the presence of the terminal hydroxyl liquid nitrile rubber improves the compatibility of the system with the hydroxyl polyolefin polymer, and improves the toughness and hydrolysis resistance of the system, reduces the strong polarity of the system, and improves the bonding performance to the weak polar substrate.
[0019] Furthermore, the thermoplastic resin is acrylic resin.
[0020] The beneficial effect of adopting the above further technical solution is that the thermoplastic acrylic resin has a high initial adhesion, which improves the initial bonding strength of the system.
[0021] Furthermore, the isocyanate is one of p-phenylene diisocyanate (PPDI), toluene diisocyanate (TDI), and diphenylmethane-4,4'-diisocyanate (MDI), preferably diphenylmethane-4,4'-diisocyanate.
[0022] Furthermore, the coupling agent is mercaptopropyl trimethoxysilane or γ-glycidyloxypropyl trimethoxysilane, preferably mercaptopropyl trimethoxysilane. The addition of the coupling agent greatly improves the adhesion of various substrates.
[0023] Furthermore, the catalyst is organic bismuth or bismorpholine diethyl ether, and the amine catalyst increases the reaction rate of isocyanate groups and moisture in the system.
[0024] The present invention also relates to a method for preparing the reactive polyurethane hot melt adhesive as described above, comprising adding crystalline polyester polyol, hydroxyl-terminated liquid nitrile rubber, and hydroxyl polyolefin polymer into a container by weight, heating until the crystalline polyester polyol is dissolved and then starting to stir, adding a thermoplastic resin while stirring, and when the temperature rises to 140-150°C, starting to evacuate and maintaining the temperature for 90 minutes, cooling the temperature to 70-90°C, adding isocyanate under nitrogen protection, reacting for 1.5-2.5 hours, adding a coupling agent and a catalyst under nitrogen protection, and stirring at 100-120°C for 30 minutes, then discharging the material under nitrogen protection, and degassing the material in a vacuum oven at 100-120°C for 20 minutes, and finally sealing and packaging.
[0025] The advantages of the present invention are:
[0026] (1) The hydroxyl polyolefin polymer used in the present invention has a hydroxyl group and a polyolefin structure, so that a polyolefin structure is introduced into the molecular structure of the reactive polyurethane hot melt adhesive, thereby improving the adhesion of the system to weakly polar substrates, which is superior to ordinary polyester polyols, polyether polyols, etc., and its hydrolysis resistance and electrical properties are particularly advantageous;
[0027] (2) The addition of hydroxyl-terminated liquid nitrile rubber improves the compatibility of hydroxyl polyolefin polymer in the system and further improves the adhesion of the product to weakly polar substrates, with obvious effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of bonding the ABS resin sheet and the ink glass;
[0029] Figure 2 Schematic diagram of the high temperature and high humidity test process.
[0030] The reference numerals are recorded as follows: 1. ABS resin sheet; 2. ink glass; 3. glue line; 4. center hole; 5. dynamometer pressure head. DETAILED DESCRIPTION
[0031] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0032] It should be noted that the “parts” mentioned in the present invention are all parts by weight.
[0033] Example 1
[0034] In a 500mL three-necked flask equipped with a thermometer, a stirring paddle and a vacuum device, 27.5 parts of crystalline polyester polyol 1,6-hexanediol adipate (HDO / AA), 17.5 parts of hydroxyl-terminated liquid nitrile rubber, and 17.5 parts of hydroxyl polyolefin polymer were added, and stirring began after heating until the crystalline polyester polyol was dissolved. 17.5 parts of thermoplastic resin (Mitsubishi BR-113) were added while stirring. When the temperature rose to 145°C, vacuum was started and maintained for 90 minutes, and then cooled to 80°C. 25 parts of isocyanate MDI were added under nitrogen protection. After reacting for 2 hours, 0.75 parts of coupling agent mercaptopropyltrimethoxysilane and 0.3 parts of catalyst bismorpholine diethyl ether were added under nitrogen protection, and stirred at 110°C for 30 minutes, then discharged under nitrogen protection, and vacuum-defoamed in a vacuum oven at 110°C for 20 minutes, and finally sealed and packaged.
[0035] Example 2
[0036] In a 500mL three-necked flask equipped with a thermometer, a stirring paddle and a vacuum device, 25 parts of crystalline polyester polyol 1,6-hexanediol adipate (HDO / AA), 20 parts of hydroxyl-terminated liquid nitrile rubber, and 15 parts of hydroxyl polyolefin polymer were added, and stirring began after heating until the crystalline polyester polyol was dissolved. 20 parts of thermoplastic resin (Mitsubishi BR-113) were added while stirring. When the temperature rose to 145°C, vacuum was started and maintained for 90 minutes, and then the temperature was lowered to 80°C. 20 parts of isocyanate MDI were added under nitrogen protection. After reacting for 2 hours, 1.0 parts of coupling agent mercaptopropyltrimethoxysilane and 0.1 parts of catalyst bismorpholine diethyl ether were added under nitrogen protection, and stirred at 110°C for 30 minutes, then discharged under nitrogen protection, and vacuum-defoamed in a vacuum oven at 110°C for 20 minutes, and finally sealed and packaged.
[0037] Example 3
[0038] In a 500mL three-necked flask equipped with a thermometer, a stirring paddle and a vacuum device, 30 parts of crystalline polyester polyol 1,6-hexanediol adipate (HDO / AA), 15 parts of hydroxyl-terminated liquid nitrile rubber, and 20 parts of hydroxyl polyolefin polymer were added, and stirring began after heating until the crystalline polyester polyol was dissolved. 15 parts of thermoplastic resin (Mitsubishi BR-113) were added while stirring. When the temperature rose to 145°C, vacuum was started and maintained for 90 minutes, and then the temperature was lowered to 80°C. 30 parts of isocyanate MDI were added under nitrogen protection. After reacting for 2 hours, 0.5 parts of coupling agent mercaptopropyltrimethoxysilane and 0.5 parts of catalyst bismorpholine diethyl ether were added under nitrogen protection, and stirred at 110°C for 30 minutes, then discharged under nitrogen protection, and vacuum-defoamed in a vacuum oven at 110°C for 20 minutes, and finally sealed and packaged.
[0039] Comparative Example 1
[0040] In a 500mL three-necked flask equipped with a thermometer, a stirring paddle and a vacuum device, 27.5 parts of crystalline polyester polyol 1,6-hexanediol adipate (HDO / AA), 17.5 parts of hydroxyl-terminated liquid nitrile rubber, and 17.5 parts of hydroxyl-terminated polyether were added, and stirring began after heating until the crystalline polyester polyol was dissolved. 17.5 parts of thermoplastic resin (Mitsubishi BR-113) were added while stirring. When the temperature rose to 145°C, vacuum was started and maintained for 90 minutes, and then cooled to 80°C. 25 parts of isocyanate MDI were added under nitrogen protection. After reacting for 2 hours, 0.75 parts of coupling agent mercaptopropyltrimethoxysilane and 0.3 parts of catalyst bismorpholine diethyl ether were added under nitrogen protection, and stirred at 110°C for 30 minutes, then discharged under nitrogen protection, and vacuum-defoamed in a vacuum oven at 110°C for 20 minutes, and finally sealed and packaged.
[0041] Comparative Example 2
[0042] In a 500mL three-necked flask equipped with a thermometer, a stirring paddle and a vacuum device, 27.5 parts of crystalline polyester polyol 1,6-hexanediol adipate (HDO / AA), 17.5 parts of liquid polyester polyol 3-methyl-1,5-pentanediol adipate (MPD / AA), and 17.5 parts of terminal hydroxyl polyether were added, and stirring began after heating until the crystalline polyester polyol was dissolved. 17.5 parts of thermoplastic resin BR-113 were added while stirring. When the temperature rose to 145°C, vacuum was started and maintained for 90 minutes, and then cooled to 80°C. 25 parts of isocyanate MDI were added under nitrogen protection. After reacting for 2 hours, 0.75 parts of coupling agent mercaptopropyltrimethoxysilane and 0.3 parts of catalyst bismorpholine diethyl ether were added under nitrogen protection, and stirred at 110°C for 30 minutes, then discharged under nitrogen protection, and vacuum-defoamed in a vacuum oven at 110°C for 20 minutes, and finally sealed and packaged.
[0043] test
[0044] Test 1: Bond strength test
[0045] The reactive polyurethane hot melt adhesive of Examples 1-3 and Comparative Examples 1-2 was subjected to a bonding strength test. The bonding interface materials were ABS resin sheet 1 and ink glass 2. The reactive polyurethane hot melt adhesive was heated to 115°C and then dispensed onto the ABS resin sheet 1 substrate with a center hole 4. The adhesive line 3 (reactive polyurethane hot melt adhesive) had a width of 1±0.2mm. The ink glass was then pressed for bonding. The thickness was 0.15mm and a pressure of 3kg was applied. After the pressure was maintained for 2 hours, the adhesive was placed in a constant temperature and humidity chamber at a temperature of 25°C and a humidity of 50% for 7 days for curing. Then, the ejection strength test was performed. The bonding schematic diagram of the ABS resin sheet and the ink glass is shown in FIG. Figure 1 .
[0046] Test 2: High temperature and high humidity test
[0047] After the samples of test 1 were cured for 7 days, they were placed in an aging box at a temperature of 65°C and a humidity of 90%, and the ejection strength test was performed according to test 1. The test process is shown in Figure 2 , the dynamometer pressure head 5 acts on the ink glass 2 through the center hole 4.
[0048] Test 3: Breakdown voltage test
[0049] According to GB T / 1408.1-2016, a sample with a thickness of 1 mm was made and placed in a constant temperature and humidity chamber at a temperature of 25°C and a humidity of 50% for curing for 7 days, and then the dielectric strength test was carried out.
[0050] See Table 1 for specific data.
[0051] Table 1 Performance data table
[0052]
[0053] It can be seen from the results in Table 1 that the ejection strength, ejection strength after high temperature and high humidity, and dielectric strength of Examples 1-3 are significantly higher than those of Comparative Examples 1 and 2.
[0054] The difference between Examples 1, 2, and 3 and Comparative Example 1 is that the polyols used are different. The hydroxyl polyolefin polymer structure in Example 1 is combined with the hydroxyl-terminated liquid nitrile rubber, and compared with the ordinary liquid polyester polyol used in Comparative Example 1 and the hydroxyl-terminated liquid nitrile rubber, it can be found from the data in Table 1 that the presence of the hydroxyl polyolefin polymer and its use in combination with the hydroxyl-terminated liquid nitrile rubber improves the product's bonding strength to weakly polar substrates, improves its high temperature and humidity resistance, and improves its dielectric strength.
[0055] Compared with Comparative Examples 1 and 2, in particular, the difference between Example 1 and Comparative Example 2 is that the combination of the hydroxyl polyolefin polymer structure and the hydroxyl-terminated liquid nitrile rubber used in Example 1 is different from the combination of the ordinary liquid polyester polyol and the ordinary polyether polyol in Comparative Example 2. It can be found from the data in Table 1 that the combination of the hydroxyl polyolefin polymer structure and the hydroxyl-terminated liquid nitrile rubber provided by the present invention is better than the combination of ordinary polyester polyol and polyether polyol. The ejection strength of the product is significantly improved, the bonding strength after high temperature and high humidity resistance decreases less, the improvement is obvious, and the dielectric strength is also significantly improved.
[0056] From the test results of the entire embodiment and the comparative example, it can be found that the coordinated use of the raw materials of the entire system of the present application improves the ejection strength, high temperature and high humidity resistance and electrical properties of the product as a whole.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a reactive polyurethane hot melt adhesive, characterized in that: In a 500mL three-necked flask equipped with a thermometer, a stirring paddle and a vacuum device, 30 parts of crystalline polyester polyol 1,6-hexanediol adipate, 15 parts of hydroxyl-terminated liquid nitrile rubber, and 20 parts of hydroxyl polyolefin polymer were added, and stirring began after heating until the crystalline polyester polyol was dissolved. 15 parts of thermoplastic resin Mitsubishi BR-113 were added while stirring. When the temperature rose to 145°C, vacuum was started and maintained for 90 minutes, and then the temperature was lowered to 80°C. 30 parts of isocyanate MDI were added under nitrogen protection. After reacting for 2 hours, 0.5 parts of coupling agent mercaptopropyl trimethoxysilane and 0.5 parts of catalyst bismorpholine diethyl ether were added under nitrogen protection, and stirred at 110°C for 30 minutes, and then the material was discharged under nitrogen protection, and the vacuum oven was vacuum-defoamed at 110°C for 20 minutes, and finally sealed and packaged; The hydroxyl polyolefin polymer has the following structure: , The value range of X is 10-22, and the value range of Y is 2-14.
Citation Information
Patent Citations
Preparation method of natural latex modified waterborne polyurethane for preparation of condoms
CN107501913A
Quickly-curing two-component reactive adhesive and preparation method thereof
CN108048023A
High-performance polyurethane hot melt adhesive and preparation method thereof
CN112662368A
Preparation method of PU adhesive, PU adhesive and method for applying PU adhesive to EPDM bonding
CN113652192A
Hot melt adhesive, raw material composition, preparation method, application and electronic element
CN114989769A