A surface coating process for composite plastics and its application

Through the composite plastic surface plating process, the internal stress is reduced by using air treatment of 65-70℃ and soaking of low-concentration acetone and ethanol solutions. Combined with electroplating technology, the problem of difficult to take into account both conductivity and anti-aging properties in plastic electroplating technology is solved, and the composite is improved The mechanical properties and electrical conductivity of plastics are suitable for mobile phone frames and other fields.

CN115874241BActive Publication Date: 2024-11-19深圳市生利科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211122337.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-11-19
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

The existing plastic electroplating technology is difficult to maintain high conductivity while maintaining good anti-aging properties. When the plastic is combined with metal, internal stress increases due to dimensional changes and differences in heat shrinkage values, resulting in product warping, deformation and cracking.

Method used

The surface plating process of composite plastics is adopted, including composite plastic preparation, prepreg treatment, oil removal, initiator treatment, catalysis and electroplating. The internal stress is reduced through air treatment at 65-70°C and soaking in low-concentration acetone and ethanol solution, and the internal stress is improved. Molecular binding force improves plating binding force and conductivity.

Benefits of technology

It significantly reduces internal stress, improves the aging resistance, mechanical properties and electrical conductivity of composite plastics, extends product life, and enhances the coverage and wear resistance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003846981070000081
    Figure BDA0003846981070000081
Patent Text Reader

Abstract

The present invention relates to C25D5, and more specifically, to a surface coating process of a composite plastic and its application. The steps are as follows: (1) preparation of composite plastic; (2) pre-dip treatment; (3) degreasing; (4) initiator treatment; (5) catalysis; (6) electroplating. Controlling the weight ratio of hydrochloric acid aqueous solution, titanium trichloride and titanium powder in the initiator to be 50: (0.5-1.4): (0.07-0.15) can not only trigger electroplating and make electroplating easier, but also promote uniform deposition of the coating, increase the covering power of the coating, and improve the mechanical ability of the coating, especially the wear resistance. The process of the present invention not only further gently reduces the internal force, improves the anti-aging ability of the final product, and prolongs its life, but also helps to improve the stability and mechanical properties of the product, and also unexpectedly improves the conductivity of the product. The surface coating process is used for a variety of metal coatings, and is particularly suitable for the field of mobile phone frames.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to C25D5, and more particularly to a surface coating process of composite plastic and application thereof. Background Art

[0002] At present, many developers have begun to use plastic materials to produce mobile phone frames due to the requirements of drop resistance and lightness. However, with the advancement of social science and technology, people have begun to have more requirements for the appearance of mobile phone frames. Traditional plastic mobile phone frames cannot have the texture of metallic luster. Therefore, the combination technology of plastic mobile phone cases and metals has attracted extensive research from scholars. The commonly used methods are mixed metal powder injection molding or electroplating on the outer surface of plastic mobile phone cases.

[0003] Patent No. CN106487970B provides an aluminum alloy plastic composite material mobile phone frame and its manufacturing method. After mixing aluminum metal powder, it is printed out by 3D printing micro-jet, and then injection molded to obtain a plastic substrate preparation, which improves the strength of the mobile phone frame and reduces pollution during the process. Patent No. CN105200669B provides a pre-treatment method for electroplating plastic parts. Nanofibers are deposited on the plastic surface to form a rough interface on the surface that is conducive to the bonding of the coating, and electroplating can be performed without roughening.

[0004] However, in these plastic electroplating technologies, the obtained coatings cannot maintain high conductivity and good anti-aging performance at the same time. Summary of the invention

[0005] In order to solve the above problems, the first aspect of the present invention provides a surface coating process for composite plastics, the steps of which are as follows: (1) preparation of composite plastics; (2) pre-immersion liquid treatment; (3) degreasing; (4) initiator treatment; (5) catalysis; and (6) electroplating.

[0006] As a preferred technical solution of the present invention, the raw materials of the composite plastic include polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN).

[0007] Preferably, the melt flow rate (300°C / 1.2kg) of the PC is 8-15g / 10min.

[0008] Preferably, the content of product glue in the ABS is 50-80wt%.

[0009] Preferably, the density of the SAN is 1-1.1 g / cm 3 .

[0010] As a preferred technical solution of the present invention, in the raw materials of the composite plastic, the weight ratio of polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN) is (42-48): (38-42): (6-9).

[0011] Preferably, in the raw materials of the composite plastic, the weight ratio of polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN) is 45:40:8.

[0012] Preferably, step (1) is to add polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN) in a weight ratio into a twin-screw extruder for granulation, and then use an injection molding machine to obtain a rectangular plate with a size of 8cm×5cm×1cm, which is a composite plastic.

[0013] As a preferred technical solution of the present invention, the pre-immersion liquid is selected from one or more of acetone aqueous solution, acetic acid aqueous solution and ethanol aqueous solution.

[0014] Preferably, the pre-soaking liquid is a mixture of an acetone aqueous solution and an ethanol aqueous solution.

[0015] Further preferably, in the pre-dip solution, the weight ratio of the acetone aqueous solution to the ethanol aqueous solution is (0.8-2):1.

[0016] More preferably, in the acetone aqueous solution, the mass fraction of acetone is 15-19 wt %; in the ethanol aqueous solution, the mass fraction of ethanol is 70-80 wt %.

[0017] Preferably, the step (2) is specifically as follows: after the composite plastic is allowed to stand in air at 65-70° C. for 1.5-2 hours, it is immersed in a pre-immersion liquid for 3-7 seconds, taken out, and rinsed with deionized water to obtain a pre-treated part.

[0018] Plastic products generally have the disadvantage of internal stress. Especially when plastics and metals are combined, the internal stress of the product is further increased due to the large difference between the dimensional change of the metal and the thermal shrinkage value of the plastics, causing warping and cracking. In order to reduce the negative impact of this internal stress, 20-25wt% acetone solution is often used in industry to treat plastics. However, this treatment method is not only very limited in reducing the internal stress, but also due to the introduction of ketone organic solvents, it may cause "spotting" on the plastic surface, thereby shortening the anti-aging ability of the product and reducing its life. The applicant has found through a large number of experiments that first using hot air treatment and then using low-concentration acetone solution and ethanol solution for soaking can not only significantly reduce the generation of the above-mentioned problems, further gently reduce the internal stress, improve the anti-aging ability of the final product, extend its life, and help improve the stability and mechanical properties of the product, in addition to unexpectedly improving the product conductivity. The applicant speculates that first treating with hot air for a certain period of time, especially treating with air at 65-70°C for 1.5-2h, can gently reduce the internal stress without damaging the plastic surface, and provide favorable bonding conditions for the subsequent pre-dip treatment. On the basis of partial stress removal, the ester bonds of PC with a specific melt flow rate, the hydrogen on the benzene ring of SAN with a specific density, the carbonyl group of the acetone aqueous solution and the hydroxyl group of the alcohol aqueous solution interact with each other in the hot plastic part, which not only improves the bonding force between molecules, but also reduces the internal stress of the plastic and avoids the generation of bubbles on its surface during electroplating, thereby improving the bonding force of the coating and improving the mechanical capacity of the product; and such interaction is also conducive to improving the dispersibility of the plastic itself, improving the electron mobility during electroplating, not only improving the conductivity of the product, but also improving the stability and anti-aging properties of the product. This effect is particularly significant when the weight ratio of polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN) is (42-48): (38-42): (6-9).

[0019] Preferably, step (3) is specifically to immerse the pre-treated part in the degreasing agent for 3-5 minutes, then immerse it in a 40-50wt% hydrochloric acid aqueous solution for 2-3 minutes, and take it out to obtain the degreasing part.

[0020] Preferably, the degreasing agent is prepared by adding sodium hydroxide, trisodium phosphate, and sodium carbonate into deionized water, so that the concentration of sodium hydroxide is 105 g / L, the concentration of trisodium phosphate is 170 g / L, and the concentration of sodium carbonate is 105 g / L.

[0021] As a preferred technical solution of the present invention, the initiator includes an acidic aqueous solution and metal powder.

[0022] As a preferred technical solution of the present invention, the acidic aqueous solution is a hydrochloric acid aqueous solution, and the metal powder is a mixture of titanium trichloride and titanium powder.

[0023] Further preferably, in the initiator, the weight ratio of the hydrochloric acid aqueous solution, titanium trichloride and titanium powder is 50:(0.5-1.4):(0.07-0.15).

[0024] More preferably, the particle size of the titanium powder is 1-20 micrometers. The hydrochloric acid aqueous solution is a hydrochloric acid aqueous solution with a mass fraction of 40-70 wt%.

[0025] Preferably, step (4) is to immerse the degreased part in a roughening liquid, react at 40-60°C for 6-8 minutes, take it out, and then immerse it in an initiator, react at 25°C for 30-40 minutes to obtain an initiating part.

[0026] As a preferred technical solution of the present invention, the catalysis includes activator treatment and degumming treatment.

[0027] As a preferred technical solution of the present invention, the activator is selected from one or more of silver nitrate, stannous chloride, palladium chloride, and 30-40wt% hydrochloric acid aqueous solution.

[0028] As a preferred technical solution of the present invention, the activator is a mixture of silver nitrate, stannous chloride, palladium chloride and 30-40wt% hydrochloric acid aqueous solution.

[0029] Preferably, in the activator, the weight ratio of silver nitrate, stannous chloride, palladium chloride and 30-40wt% hydrochloric acid aqueous solution is (0.08-0.12):(0.5-0.7):(0.1-0.4):(45-70).

[0030] Preferably, the activator treatment is specifically to immerse the initiator into the activator, react at 20-30° C. for 2-3 minutes, to obtain the activated part.

[0031] Preferably, the debonding treatment is specifically to immerse the activated part in a 3-4 wt % hydrochloric acid aqueous solution for 1-2 min to obtain a debonded part.

[0032] As a preferred technical solution of the present invention, the electroplating is selected from one or more of copper electroplating, nickel electroplating and chromium electroplating.

[0033] Preferably, the electroplating is copper electroplating.

[0034] Further preferably, the copper electroplating is specifically to place the debonded part into an electroplating tank containing an electroplating solution, and electroplate at 50-60° C. for 10-30 minutes to obtain an electroplated product.

[0035] The preparation method of the electroplating solution is as follows: copper pyrophosphate, potassium pyrophosphate and copper pyrophosphate solution are added to deionized water, so that the concentration of copper pyrophosphate is 80-90 g / L, the concentration of potassium pyrophosphate is 300-320 g / L, and the concentration of copper pyrophosphate solution is 2-4 mL / L. Ammonia water is continuously added to adjust the pH of the solution to 8.5-9, and the electroplating solution is obtained.

[0036] A second aspect of the present invention provides an application of a surface coating process of a composite plastic, wherein the surface coating process of the composite plastic is applied to a mobile phone frame.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] First treat with air at 65-70°C for 1.5-2h, then soak the composite plastic in an acetone aqueous solution and an ethanol aqueous solution at a weight ratio of (0.8-2):1, which not only further gently reduces the internal force, improves the anti-aging ability of the final product, and prolongs its life, but also helps to improve the stability and mechanical properties of the product, and unexpectedly improves the conductivity of the product. Controlling the weight ratio of hydrochloric acid aqueous solution, titanium trichloride and titanium powder in the initiator to 50: (0.5-1.4): (0.07-0.15) can not only trigger electroplating and make electroplating easier, but also promote uniform deposition of the coating, increase the covering power of the coating, and improve the mechanical ability of the coating, especially the wear resistance. The process of the present invention can be used not only for copper plating, but also for various metal plating such as nickel plating and chromium plating, thereby improving the conductivity and stability of composite plastic electroplated products. The obtained electroplated products are particularly suitable for the field of mobile phone frames. DETAILED DESCRIPTION

[0039] Example

[0040] The raw materials for preparing the composition in the embodiment are all commercially available, wherein PC is purchased from Sabre with the brand name EXL9330 and the melt flow rate (300°C / 1.2kg) of 10g / 10min, ABS is purchased from Shandong Wanda with the name ABS high rubber powder with the brand name WD-132 and the product rubber content of 55-70wt%, and SAN is purchased from Daqing Petrochemical with the brand name SAN-327 (extrusion grade) and the density of 1.06-1.08g / cm 3 Titanium powder was purchased from Wuxi Qianbai Materials Technology Co., Ltd. with a particle size of 2-3 μm. Coarsening liquid was purchased from Shenzhen Shengli Technology Co., Ltd. with a model of SL-525. Coke solution was purchased from Bigley with a model of Cu-203.

[0041] Example 1

[0042] This example provides a surface coating process for composite plastics, the steps of which are as follows: (1) preparation of composite plastics; (2) pre-immersion liquid treatment; (3) degreasing; (4) initiator treatment; (5) catalysis; and (6) electroplating.

[0043] The raw materials of the composite plastic include polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN). In the raw materials of the composite plastic, the weight ratio of polycarbonate, acrylonitrile-butadiene-styrene plastic and styrene acrylonitrile plastic is 45:40:8.

[0044] Step (1) specifically comprises adding polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN) according to weight ratio into a twin-screw extruder for granulation, and then using an injection molding machine to obtain a rectangular plate with a size of 8 cm×5 cm×1 cm, i.e., a composite plastic.

[0045] The pre-soaking liquid is a mixture of an acetone aqueous solution and an ethanol aqueous solution, wherein the weight ratio of the acetone aqueous solution to the ethanol aqueous solution in the pre-soaking liquid is 1.3:1.

[0046] In the acetone aqueous solution, the mass fraction of acetone is 17wt%; in the ethanol aqueous solution, the mass fraction of ethanol is 75wt%.

[0047] The step (2) is specifically as follows: after the composite plastic is allowed to stand in air at 67° C. for 1.8 hours, it is immersed in 500 mL of pre-immersion liquid for 5 seconds, taken out, and rinsed with 1 L of deionized water to obtain a pre-treated part.

[0048] Step (3) specifically comprises soaking the pre-treated part in 1L of degreasing agent for 4 minutes, then soaking it in 1L of 45wt% hydrochloric acid aqueous solution for 2 minutes, and taking it out to obtain a degreasing part.

[0049] The degreasing agent is prepared by adding sodium hydroxide, trisodium phosphate, and sodium carbonate into deionized water, so that the concentration of sodium hydroxide is 105 g / L, the concentration of trisodium phosphate is 170 g / L, and the concentration of sodium carbonate is 105 g / L.

[0050] Initiators include acidic aqueous solutions and metal powders.

[0051] The acidic aqueous solution is a hydrochloric acid aqueous solution, and the metal powder is a mixture of titanium trichloride and titanium powder.

[0052] The initiator is a mixture of hydrochloric acid aqueous solution, titanium trichloride and titanium powder. In the initiator, the weight ratio of hydrochloric acid aqueous solution, titanium trichloride and titanium powder is 50:0.8:0.09.

[0053] The hydrochloric acid aqueous solution is a hydrochloric acid aqueous solution with a mass fraction of 50 wt%.

[0054] Step (4) specifically comprises immersing the degreased part in 500 mL of roughening liquid, reacting at 50° C. for 6 min, taking it out, and then immersing it in 500 mL of initiator, reacting at 25° C. for 30 min to obtain an initiating part.

[0055] Catalysis includes activator treatment and debonding treatment.

[0056] The activator is a mixture of silver nitrate, stannous chloride, palladium chloride and 35 wt % hydrochloric acid aqueous solution.

[0057] In the activator, the weight ratio of silver nitrate, stannous chloride, palladium chloride and 35wt% hydrochloric acid aqueous solution is 0.1:0.6:0.2:60.

[0058] The activator treatment is specifically as follows: the initiator is immersed in 500 mL of the activator, reacted at 25° C. for 2 minutes, and an activated part is obtained.

[0059] The debonding treatment is specifically to immerse the activated part in 500 mL of 4 wt % hydrochloric acid aqueous solution for 2 minutes to obtain a debonded part.

[0060] The electroplating is copper electroplating.

[0061] The copper electroplating is specifically as follows: placing the debonded part into an electroplating tank containing 1 L of electroplating solution, electroplating at 54° C. for 20 minutes to obtain an electroplated product.

[0062] The preparation method of the electroplating solution is as follows: copper pyrophosphate, potassium pyrophosphate and copper pyrophosphate solution are added to deionized water, so that the concentration of copper pyrophosphate is 84 g / L, the concentration of potassium pyrophosphate is 315 g / L, and the concentration of copper pyrophosphate solution is 3 mL / L. Ammonia water is continuously added to adjust the pH of the solution to 8.7, and the electroplating solution is obtained.

[0063] Example 2

[0064] This example provides a surface coating process for composite plastics, which is different from Example 1 in that the weight ratio of polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN) in the raw materials of the composite plastics is 44:40:7. The pre-dip solution is a mixture of acetone aqueous solution and ethanol aqueous solution.

[0065] In the pre-soaking solution, the weight ratio of the acetone aqueous solution to the ethanol aqueous solution is 0.9:1, the mass fraction of acetone in the acetone aqueous solution is 18wt%; and the mass fraction of ethanol in the ethanol aqueous solution is 75wt%.

[0066] In the activator, the weight ratio of silver nitrate, stannous chloride, palladium chloride and 34wt% hydrochloric acid aqueous solution is 0.08:0.6:0.15:50.

[0067] Example 3

[0068] This example provides a surface coating process for composite plastics. Different from Example 1, the preparation method of the electroplating solution is as follows: copper pyrophosphate, potassium pyrophosphate and copper pyrophosphate solution are added to deionized water, so that the concentration of copper pyrophosphate is 80 g / L, the concentration of potassium pyrophosphate is 300 g / L, and the concentration of copper pyrophosphate solution is 4 mL / L. Ammonia water is continuously added to adjust the pH of the solution to 9, thereby obtaining the electroplating solution.

[0069] The copper electroplating process specifically includes placing the debonded part into an electroplating tank filled with electroplating solution and electroplating at 60° C. for 17 minutes.

[0070] Example 4

[0071] This example provides a surface coating process for composite plastics, which is different from Example 1 in that the weight ratio of polycarbonate (PC), acrylonitrile-butadiene-styrene plastic (ABS) and styrene acrylonitrile plastic (SAN) in the raw materials of the composite plastics is 43:39:7. The pre-dip solution is a mixture of acetone aqueous solution and ethanol aqueous solution.

[0072] In the pre-soaking solution, the weight ratio of the acetone aqueous solution to the ethanol aqueous solution is 0.5:1, the mass fraction of acetone in the acetone aqueous solution is 19wt%; and the mass fraction of ethanol in the ethanol aqueous solution is 70wt%.

[0073] The copper electroplating step specifically involves placing the debonded part into an electroplating tank filled with electroplating solution and electroplating at 52° C. for 25 minutes.

[0074] Example 5

[0075] This example provides a surface coating process for composite plastics. The difference from Example 1 is that the initiator is a mixture of hydrochloric acid aqueous solution, titanium trichloride and titanium powder. In the initiator, the weight ratio of hydrochloric acid aqueous solution, titanium trichloride and titanium powder is 50:2:0.05.

[0076] The copper electroplating step specifically involves placing the debonded part into an electroplating tank filled with electroplating solution and electroplating at 56° C. for 20 minutes.

[0077] Performance Test:

[0078] 1. Average electroplating peeling force test: The electroplated products obtained in Examples 1-5 were respectively tested for peeling force using a peeling instrument at a test speed of 100 mm / min to obtain a force-distance curve. The average value of the platform area was taken as the average electroplating peeling force. The results are shown in Table 1:

[0079] Table 1

[0080] Example Average plating stripping force (N) 1 9.4 2 9.1 3 9.3 4 7.5 5 7

[0081] 2. Rubber friction test: The electroplated products obtained in Examples 1-5 were subjected to a load of 600g, and an experimental rubber (purchased from SEEDER, model 510) was used to rub the surface of the electroplated products back and forth for 100 cycles. The side edges were rubbed for 50 cycles, 30 times per minute, and the stroke was 4cm. The rubber could not be separated from the sample. Observe and record whether the coating fell off and whether the base material was exposed. Among them, the coating at the wear-resistant part did not fall off and the base material was not exposed, which was qualified, otherwise it was unqualified. Each example was set with 10 parallel samples, and the qualified number was recorded. The results are shown in Table 2:

[0082] Table 2

[0083]

[0084]

[0085] 3. Resistance test: The electroplated products obtained in Examples 1-5 were tested for resistance according to GB / T 6146-2010, wherein resistance R<1Ω was recorded as level 1, 1Ω≤resistance R≤1.5Ω was recorded as level 2, and 1.5Ω<resistance R≤2Ω was recorded as level 3. The results are shown in Table 3:

[0086] Table 3

[0087] Example Resistance Value 1 Level 1 2 Level 1 3 Level 1 4 Level 2 5 Level 2

[0088] 4. Pencil hardness test: The electroplated plastic primary products obtained in Examples 1-5 were scratched with a Mitsubishi pencil (UNI series) at an angle of 45 degrees and a load of 500 gf on the sample surface from different directions with 3 lines of 1.0±0.2 cm in length. After erasing the pencil marks with an eraser, the pencils were tested one by one from the hardest pencil in order from hard to soft until the coating was found to be unscratched. The hardness value at this time was recorded, wherein a hardness value ≥7H was A, a hardness value 5≤<7 was B, a hardness value 4≤<5 was C, and a hardness value <4H was D. The results are shown in Table 4:

[0089] Table 4

[0090] Example Pencil hardness test 1 A 2 B 3 B 4 C 5 B

[0091] 5. Ultraviolet aging test: The electroplated product obtained in Example 1-5 was covered with black adhesive tape on one side, and the lamp power was set to 0.63 W / m 2 , put the sample in the test box, at a temperature of 65℃, direct ultraviolet light on the side not stuck with black tape, irradiate for 5 hours, and then place it at 45℃ for 4 hours, this is one cycle. After 15 cycles, take out the sample, leave it at 25℃ for 5 hours, and then observe the surface of the side of the electroplated product not stuck with black tape. The results are shown in Table 4:

[0092] Table 5

[0093] Example UV aging test 1 No fading, no discoloration, no lines, no cracks, no peeling on the surface 2 No fading, no discoloration, no lines, no cracks, no peeling on the surface 3 No fading, no discoloration, no lines, no cracks, no peeling on the surface 4 Surface fading, discoloration, no lines, no cracks, no peeling 5 The surface has no fading, no discoloration, no lines, no cracks, and no peeling

[0094] 6. Internal stress immersion test: The electroplated products obtained in Examples 1-5 were placed in a mixture of ethyl acetate and methanol (the mass ratio of ethyl acetate to methanol in the mixture was 2:3) and immersed for 20 minutes. After being taken out, they were rinsed with 1L of water. The surface of the product was observed. Those without cracks were recorded as qualified, and those with cracks were recorded as unqualified. Ten parallel samples were set for each example, and the number of qualified samples was recorded. The results are shown in Table 6:

[0095] Table 6

[0096] Example Internal stress immersion test 1 10 2 10 3 10 4 5 5 6

Claims

1. A surface coating process for composite plastics, characterized in that: The steps are as follows: (1) preparation of composite plastic; (2) pre-impregnation liquid treatment; (3) degreasing; (4) initiator treatment; (5) catalysis; (6) electroplating; The raw materials of the composite plastic include polycarbonate, acrylonitrile-butadiene-styrene plastic and styrene acrylonitrile plastic; in the raw materials of the composite plastic, the weight ratio of polycarbonate, acrylonitrile-butadiene-styrene plastic and styrene acrylonitrile plastic is 45:40:8; Step (1) specifically comprises adding polycarbonate, acrylonitrile-butadiene-styrene plastic and styrene-acrylonitrile plastic into a twin-screw extruder according to a weight ratio for granulation, and then using an injection molding machine to obtain a rectangular plate with a size of 8 cm×5 cm×1 cm, i.e., a composite plastic; The pre-soaking liquid is a mixture of an acetone aqueous solution and an ethanol aqueous solution; in the pre-soaking liquid, the weight ratio of the acetone aqueous solution to the ethanol aqueous solution is 1.3:1; In the acetone aqueous solution, the mass fraction of acetone is 17wt%; in the ethanol aqueous solution, the mass fraction of ethanol is 75wt%; The step (2) specifically comprises placing the composite plastic under air conditions at 67° C. for 1.8 hours, immersing it in 500 mL of pre-immersion liquid for 5 seconds, taking it out, and rinsing it with 1 L of deionized water to obtain a pre-treated part; Step (3) specifically comprises soaking the pre-treated part in 1L of degreasing agent for 4 minutes, then soaking it in 1L of 45wt% hydrochloric acid aqueous solution for 2 minutes, and taking it out to obtain a degreased part; The degreasing agent is prepared by adding sodium hydroxide, trisodium phosphate and sodium carbonate into deionized water, so that the concentration of sodium hydroxide is 105 g / L, the concentration of trisodium phosphate is 170 g / L, and the concentration of sodium carbonate is 105 g / L; The initiator includes an acidic aqueous solution and a metal powder; The acidic aqueous solution is a hydrochloric acid aqueous solution, and the metal powder is a mixture of titanium trichloride and titanium powder. The initiator is a mixture of hydrochloric acid aqueous solution, titanium trichloride and titanium powder; in the initiator, the weight ratio of hydrochloric acid aqueous solution, titanium trichloride and titanium powder is 50:0.8:0.09; The hydrochloric acid aqueous solution is a hydrochloric acid aqueous solution with a mass fraction of 50wt%; Step (4) specifically comprises immersing the degreased part in 500 mL of roughening liquid, reacting at 50° C. for 6 min, taking it out, and then immersing it in 500 mL of initiator, reacting at 25° C. for 30 min, to obtain an initiating part; Catalysis includes activator treatment and degumming treatment; The activator is a mixture of silver nitrate, stannous chloride, palladium chloride, and 35 wt% hydrochloric acid aqueous solution; In the activator, the weight ratio of silver nitrate, stannous chloride, palladium chloride and 35wt% hydrochloric acid aqueous solution is 0.1:0.6:0.2:60; The activator treatment is specifically as follows: the initiator is immersed in 500 mL of the activator, reacted at 25° C. for 2 minutes, and an activated part is obtained; The debonding treatment is specifically to immerse the activated part in 500 mL of 4 wt % hydrochloric acid aqueous solution for 2 min to obtain a debonded part; The electroplating is copper electroplating; The copper electroplating is specifically as follows: placing the debonded part into an electroplating tank containing 1L of electroplating solution, electroplating at 54°C for 20 minutes, and obtaining an electroplated product; The preparation method of the electroplating solution is as follows: add copper pyrophosphate, potassium pyrophosphate and copper pyrophosphate solution into deionized water, so that the concentration of copper pyrophosphate is 84 g / L, the concentration of potassium pyrophosphate is 315 g / L, and the concentration of copper pyrophosphate solution is 3 mL / L; continue to add ammonia water to adjust the pH of the solution to 8.7 to obtain the electroplating solution.

2. An application of the surface coating process of the composite plastic according to claim 1, wherein the surface coating process of the composite plastic is applied to a mobile phone frame.