Composition for phenolic fiber modification, flexible thermal insulation material and preparation method
By modifying the phenolic fibers with polyphosphazene derivatives, the instability problem under ultraviolet light and heat is solved, the mechanical and flame retardant properties are improved, and the insulation material performance requirements of solid rocket engines are met.
Patent Information
- Application Number
- CN202211610652.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-12
AI Technical Summary
Phenolic fibers are unstable under ultraviolet light or heat, which affects their ablation resistance and mechanical properties, resulting in poor performance in thermal insulation materials applications.
The surface modification of the phenolic fibers by using specific alkoxy and/or aryloxy-substituted polyphosphazene derivatives, reduces its structural defects, improves compatibility and interface binding with rubber, enhances the ultraviolet rays of the fibers and Thermal stability.
It significantly improves the mechanical properties, flame retardant and ablation resistance of phenolic fibers, meets the performance requirements of solid rocket engines for insulating layer materials, and expands the application field of fiber-reinforced rubber.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation materials, and in particular to a composition for modifying phenolic fiber, a flexible thermal insulation material and a preparation method thereof. Background Art
[0002] With the continuous development of aerospace technology, the research on thermal protection materials has also received extensive attention from researchers. As a new type of thermal protection material, flexible, highly flame-retardant and ablation-resistant composite materials have been widely used in solid rocket engine casing materials. At present, the main materials used as the inner insulation layer matrix materials at home and abroad are nitrile rubber (NBR) system, ethylene propylene diene monomer rubber (EPDM) system, silicone rubber (SBR) system and polyphosphazene rubber (PZ) system. Among them, nitrile rubber is a commonly used rocket engine inner insulation material. It has good compatibility with metals, is easy to carbonize under high temperature conditions, and has good ablation resistance. However, with the enhancement of people's environmental awareness and the recognition of asbestos carcinogenicity, the elimination of traditional nitrile rubber / asbestos insulation layer systems has become an inevitable trend. EPDM has excellent heat resistance, aging resistance, chemical corrosion resistance and low density. However, EPDM itself has poor ablation resistance and interface bonding strength with metals, and it is necessary to add a variety of additives to improve its practical application performance. Silicone rubber has good thermal stability, high temperature resistance, low smoke and low residue. Compared with EPDM, it is easier to form a dense and strong silicon carbon layer at high temperature. However, due to the non-polar structure of silicone rubber itself, its mechanical properties and bonding properties are poor. As a new type of thermal insulation material, polyphosphazene has the advantages of good ablation resistance and erosion resistance, excellent bonding performance with metal, etc., and has broader application prospects in the future.
[0003] At present, fiber-reinforced insulation materials are widely used at home and abroad to prepare ablation-resistant composite materials, and have been successfully applied to insulation materials of various types of solid rocket engines. Among them, phenolic fiber is widely used in the field of insulation materials because of its excellent flame retardancy, high temperature stability, and good ablation resistance. However, there are the following problems in the application of phenolic fiber: the presence of a large number of phenolic hydroxyl groups in the phenolic fiber structure will cause it to be unstable under ultraviolet light or heat, affecting the improvement of the ablation resistance of the product, and easily leading to a decrease in the mechanical properties of the rubber. Therefore, it is of great significance to develop a new type of phenolic fiber reinforced flexible insulation material. Summary of the invention
[0004] In view of the poor ablation resistance and mechanical properties of phenolic fiber reinforced rubber materials in the prior art, the present invention provides a composition for phenolic fiber modification, a flexible thermal insulation material and a preparation method. The present invention uses a specific polyphosphazene derivative to perform surface modification on phenolic fiber, thereby reducing the structural defects of phenolic fiber, effectively improving the stability of phenolic fiber under ultraviolet and heat effects, and significantly improving the compatibility of the modified phenolic fiber with rubber, thereby effectively improving the mechanical properties, flame retardancy and ablation resistance of the thermal insulation material, and meeting the performance requirements of the solid rocket engine for the thermal insulation layer material.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] A composition for modifying phenolic fiber, comprising the following components in parts by weight: 80-100 parts of a polyphosphazene derivative, 10-60 parts of a reinforcing agent, 1-10 parts of an activator, 1-10 parts of a plasticizer, 1-10 parts of a vulcanizing agent, and 100-200 parts of an organic solvent;
[0007] Wherein, the polyphosphazene derivative is a polyphosphazene substituted with an alkoxy group and / or an aryloxy group;
[0008] The aryloxy group is phenoxy, 4-ethylphenoxy, 2-methoxy-4-(2-propenyl)phenoxy, 4-propenyl-2-methoxyphenoxy, 2-allylphenoxy, 5',5-diallyl-2,2'-biphenyldioxy or 4-allyl-2,6-dimethoxyphenoxy;
[0009] The alkoxy group is ethoxy, trifluoroethoxy or octafluoropentyloxy.
[0010] Compared with the prior art, the composition for modifying phenolic fiber provided by the present invention selects specific alkoxy and / or aryloxy substituted polyphosphazene derivatives to modify the phenolic fiber, and by coating a layer of polyphosphazene derivatives on the surface of the phenolic fiber, the interfacial compatibility between the rubber matrix and the phenolic fiber is improved, and the dispersibility of the phenolic fiber in the rubber is improved; and by adding a vulcanizing agent to the composition, the phenolic fiber and the rubber matrix can be co-vulcanized, and the wettability of the rubber matrix on the surface of the phenolic fiber is effectively improved, thereby effectively improving the interfacial bonding force between the phenolic fiber and the rubber matrix through mechanical interlocking force, thereby improving the structural stability of the fiber-reinforced rubber; in addition, the use of specific polyphosphazene derivatives to modify the phenolic fiber can also reduce the structural defects of the phenolic fiber, improve the ultraviolet and thermal stability of the phenolic fiber, and help to improve the strength of the phenolic fiber, so that the modified phenolic fiber can significantly improve the mechanical properties, ablation resistance and flame retardancy of the rubber, which is of great significance for expanding the application field of fiber-reinforced rubber.
[0011] It should be noted that the phenolic fiber in the present invention can be short-cut fiber or fiber fabric.
[0012] Preferably, the preparation method of the polyphosphazene derivative comprises:
[0013] Step 1: adding the aromatic phenol and / or organic alcohol dropwise to a tetrahydrofuran solution of metallic sodium, reacting at 20-40° C. for 6 h-24 h to obtain an organic sodium salt;
[0014] Step 2, adding the organic sodium salt to a tetrahydrofuran solution of polydichlorophosphazene, reacting at 115° C.-125° C. for 6 h-24 h, removing the solvent, and drying to obtain the polyphosphazene derivative;
[0015] The aromatic phenol is phenol, 4-ethylphenol, eugenol, isoeugenol, 2-allylphenol, magnolol or 4-allyl-2,6-dimethoxyphenol; the organic alcohol is ethanol, trifluoroethanol or octafluoropentanol.
[0016] In combination with the above, in step 1, the mass ratio of the aromatic phenol and / or organic alcohol, metallic sodium, and tetrahydrofuran is 4-6:1:95-105.
[0017] Furthermore, in step 1, the mass ratio of the aromatic phenol and / or organic alcohol, metallic sodium and tetrahydrofuran is 5:1:100.
[0018] In combination with the above, in step 2, the mass ratio of the organic sodium salt, the polydichlorophosphazene and tetrahydrofuran is 1:1.5-2.5:15-20.
[0019] Furthermore, in step 2, the mass ratio of the organic sodium salt, polydichlorophosphazene and tetrahydrofuran is 1:2:18.
[0020] The preferred reaction conditions are conducive to the full reaction of the reaction raw materials and improve the yield of the target product.
[0021] Preferably, the reinforcing agent is white carbon black.
[0022] Preferably, the activator is zinc oxide.
[0023] Preferably, the plasticizer is stearic acid.
[0024] Preferably, the vulcanizing agent is dicumyl peroxide.
[0025] Preferably, the organic solvent is at least one of tetrahydrofuran, xylene, acetone, ethanol or dioxane.
[0026] In a second aspect, the present invention further provides a polyphosphazene-modified phenolic fiber, which is obtained by modifying the phenolic fiber with any of the above-mentioned compositions.
[0027] In a third aspect, the present invention further provides a method for preparing the polyphosphazene-modified phenolic fiber, comprising the following steps:
[0028] Step a, weighing each component according to the designed ratio of the composition described in any one of the above items, and mixing the weighed components uniformly to obtain a modified solution;
[0029] Step b, impregnating the phenolic fiber or phenolic fiber fabric with the modification solution, and drying to obtain polyphosphazene modified phenolic fiber.
[0030] Further, in combination with the above, in step b, the immersion temperature is 25°C-100°C, and the immersion time is 1 min-10 min.
[0031] Further, in combination with the above, in step b, the bath ratio of the phenolic fiber or phenolic fiber fabric to the modified solution is 1:5-50.
[0032] Further, in combination with the above, in step b, the drying temperature is 25°C-100°C, and the drying time is 50min-100min.
[0033] It should be noted that if the phenolic fiber is a long fiber, the long fiber needs to be chopped short after modification, and the length of the chopped fiber is 3mm-9mm.
[0034] In a fourth aspect, the present invention provides a flexible thermal insulation material comprising the following raw material components in parts by weight: 80-100 parts of an insulation material matrix, 1-10 parts of an activator, 20-60 parts of a reinforcing agent, 10-60 parts of a heat-resistant filler, 1-10 parts of a vulcanization aid and 5-90 parts of the above-mentioned polyphosphazene modified phenolic fiber.
[0035] The flexible thermal insulation material provided by the present invention selects the above-mentioned polyphosphazene modified phenolic fiber as the ablation-resistant fiber skeleton material. When encountering high-temperature combustion, the polyphosphazene modified phenolic fiber can be effectively converted into a dense and thick carbon fiber layer, which plays a skeleton role in connecting the carbon layer of the matrix, reduces the shedding of the carbon layer, and ensures the integrity of the structure of the thermal insulation material; in addition, the thermal conductivity of the polyphosphazene modified phenolic fiber is relatively low, thereby reducing the thermal conductivity of the thermal insulation material and the generated carbonized layer, thereby effectively improving the ablation resistance and erosion resistance of the thermal insulation material, and the presence of phenolic fiber can also significantly improve the tensile strength of the rubber matrix; furthermore, with the synergistic effect of various additives, the flame retardancy, ablation resistance, erosion resistance and mechanical properties of the thermal insulation material are significantly improved, and it has broad application prospects in the field of solid rocket engine thermal insulation materials.
[0036] Preferably, the thermal insulation matrix material is at least one of polyphosphazene rubber, EPDM rubber, nitrile rubber or silicone rubber.
[0037] Further preferably, the thermal insulation matrix material is polyphosphazene rubber.
[0038] Preferably, the activator is at least one of zinc oxide, magnesium oxide, zinc methacrylate, zinc stearate or magnesium stearate.
[0039] Preferably, the reinforcing agent is at least one of white carbon black, carbon black or modified white carbon black.
[0040] Furthermore, the modified silica is a coupling agent-modified silica, and any silica modified with a conventional coupling agent in the art can be used as the reinforcing agent of the present invention.
[0041] Preferably, the heat-resistant filler is at least one of silicon dioxide, phenolic resin, epoxy resin, silicon carbide, aluminum oxide, antimony trioxide, boric acid, zinc borate, aluminum hydroxide or boron nitride.
[0042] The preferred heat-resistant filler can improve the strength and heat resistance of the rubber matrix.
[0043] Preferably, the vulcanization aid includes at least one of sulfur, dicumyl peroxide or benzoyl peroxide.
[0044] The preferred vulcanization aid can increase the vulcanization speed, improve the compression deformation resistance and air aging resistance of the rubber matrix, and the tensile strength of the formed cross-linked body is high.
[0045] In a fifth aspect, the present invention further provides a method for preparing the flexible thermal insulation material described in any one of the above items, comprising the following steps:
[0046] The components are weighed according to the designed proportions, compounded, hot-pressed and vulcanized to obtain the flexible thermal insulation material.
[0047] Preferably, if the polyphosphazene-modified phenolic fiber is a short fiber, the weighed components are added to an open mill for blending, kneading evenly, thinning out a sheet, and hot pressing and vulcanizing to obtain the flexible thermal insulation material;
[0048] If the polyphosphazene-modified phenolic fiber is a fiber fabric, the weighed insulation material matrix, activator, reinforcing agent, heat-resistant filler and vulcanization aid are added to an open mill for blending, and the mixing is uniform and thinned out to obtain a film; after the polyphosphazene-modified phenolic fiber is cut into the same size as the film, it is placed between two films, hot-pressed and vulcanized to obtain the flexible insulation material.
[0049] Preferably, the mixing temperature in the open mixer is 20°C-40°C.
[0050] Preferably, the temperature of hot pressing vulcanization is 150°C-180°C, the pressure is 0-20MPa, and the time is t 90 min-t100 min.
[0051] The flexible thermal insulation material provided by the present invention selects polyphosphazene-modified phenolic fiber as a reinforcing material, which effectively improves the interface bonding performance between the phenolic fiber and the rubber matrix. At the same time, it is conducive to achieving continuous high carbonization and synergistically coordinating with various additives to effectively improve the flame retardancy, ablation resistance and mechanical properties of the thermal insulation material. The preparation method is simple and can be industrialized, and has broad application prospects in the field of solid rocket engine thermal insulation materials. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0053] In order to better illustrate the present invention, further examples are given below.
[0054] In the following examples, the test standards for tensile strength and elongation at break are GB / T 528-2009, and the test standards for line ablation rate and mass ablation rate are GJB 323A-96.
[0055] Example 1
[0056] The embodiment of the present invention provides a composition for modifying phenolic fiber, comprising the following raw material components in parts by weight: 90 parts of a phenoxy-substituted polyphosphazene derivative, 30 parts of white carbon black, 10 parts of zinc oxide, 10 parts of stearic acid, 3 parts of dicumyl peroxide and 200 parts of tetrahydrofuran.
[0057] The preparation method of the above-mentioned phenoxy substituted polyphosphazene derivative comprises the following steps:
[0058] Weigh 50 g of phenol and add it dropwise to a solution of sodium metal in tetrahydrofuran (10 g of sodium metal and 1000 g of tetrahydrofuran), react at room temperature for 24 h, remove the solvent by rotary evaporation, and dry to obtain sodium phenolate;
[0059] Weigh 25 g of the sodium phenolate prepared above, add it to 500 g of a tetrahydrofuran solution of polydichlorophosphazene (50 g of polydichlorophosphazene, 450 g of tetrahydrofuran), react at 120° C. for 10 h, cool, remove the solvent by rotary evaporation, and dry to obtain a phenoxy-substituted polyphosphazene derivative.
[0060] The method for modifying phenolic fiber using the above composition comprises the following steps:
[0061] Step a, weighing each component according to the designed ratio of the above-mentioned composition, and mixing the weighed components uniformly to obtain a modified solution;
[0062] Step b, immersing the phenolic fiber in the modified solution at room temperature, with a bath ratio of 1:20, an immersion time of 6 minutes, drying at 75° C. to constant weight, and chopping the phenolic fiber into short pieces, with the length of the chopped fibers being 3 mm, to obtain polyphosphazene modified phenolic fiber.
[0063] This embodiment also provides a flexible thermal insulation material, comprising the following raw material components in parts by weight: 100 parts of nitrile rubber, 10 parts of zinc oxide, 50 parts of white carbon black, 30 parts of phenolic resin, 2 parts of diisopropylbenzene peroxide and 20 parts of the polyphosphazene modified phenolic fiber prepared above.
[0064] The preparation method of the above-mentioned flexible thermal insulation material comprises the following steps:
[0065] Weigh each component according to the above ratio, add each component into an open mill, mix at 30°C, mix evenly, thin out a sheet, and hot press vulcanize. The hot press vulcanization temperature is 170°C, the pressure is 10MPa, and the time is t 95 min, to obtain the flexible thermal insulation material.
[0066] The flexible thermal insulation material prepared in this embodiment has a tensile strength of 21.3 MPa, an elongation at break of 815%, a linear ablation rate of 0.027 mm / s, and a mass ablation rate of 0.022 g / s.
[0067] Example 2
[0068] An embodiment of the present invention provides a composition for modifying phenolic fiber, comprising the following raw material components in parts by weight: 95 parts of 2-methoxy-4-(2-propenyl)phenoxy substituted polyphosphazene derivative, 40 parts of white carbon black, 5 parts of zinc oxide, 4 parts of stearic acid, 1 part of diisopropylbenzene peroxide and 130 parts of xylene.
[0069] The preparation method of the above-mentioned 2-methoxy-4-(2-propenyl)phenoxy substituted polyphosphazene derivative comprises the following steps:
[0070] Weigh 50 g of eugenol and add it dropwise to a solution of sodium metal in tetrahydrofuran (10 g of sodium metal and 1000 g of tetrahydrofuran), react at room temperature for 24 h, remove the solvent by rotary evaporation, and dry to obtain sodium eugenol;
[0071] Weigh 25 g of the sodium eugenol prepared above, add it to 500 g of a tetrahydrofuran solution of polydichlorophosphazene (50 g of polydichlorophosphazene, 450 g of tetrahydrofuran), react at 120° C. for 10 h, cool, remove the solvent by rotary evaporation, and dry to obtain a 2-methoxy-4-(2-propenyl)phenoxy substituted polyphosphazene derivative.
[0072] The method for modifying phenolic fiber using the above composition comprises the following steps:
[0073] Step a, weighing each component according to the designed ratio of the above-mentioned composition, and mixing the weighed components uniformly to obtain a modified solution;
[0074] Step b, immersing the phenolic fiber in the modified solution at room temperature, with a bath ratio of 1:15, an immersion time of 7 minutes, drying at 75° C. to constant weight, and chopping the phenolic fiber, with the length of the chopped fiber being 9 mm, to obtain polyphosphazene modified phenolic fiber.
[0075] This embodiment also provides a flexible thermal insulation material, comprising the following raw material components in parts by weight: 90 parts of EPDM rubber, 7 parts of zinc oxide, 40 parts of white carbon black, 50 parts of phenolic resin, 3 parts of diisopropylbenzene peroxide and 20 parts of the polyphosphazene modified phenolic fiber prepared above.
[0076] The preparation method of the above-mentioned flexible thermal insulation material comprises the following steps:
[0077] Weigh each component according to the above ratio, add each component into an open mill, mix at 20°C, mix evenly, thin out a sheet, and hot press vulcanize. The hot press vulcanization temperature is 150°C, the pressure is 20MPa, and the time is t 95 min, to obtain the flexible thermal insulation material.
[0078] The flexible thermal insulation material prepared in this embodiment has a tensile strength of 19.3 MPa, an elongation at break of 670%, a linear ablation rate of 0.021 mm / s, and a mass ablation rate of 0.024 g / s.
[0079] Example 3
[0080] An embodiment of the present invention provides a composition for modifying phenolic fiber, comprising the following raw material components in parts by weight: 100 parts of 5',5-diallyl-2,2'-biphenyldioxy substituted polyphosphazene derivatives, 60 parts of white carbon black, 1 part of zinc oxide, 6 parts of stearic acid, 5 parts of diisopropyl peroxide and 160 parts of acetone.
[0081] The preparation method of the above 5',5-diallyl-2,2'-biphenyldioxy substituted polyphosphazene derivative comprises the following steps:
[0082] Weigh 50 g of magnolol and add it dropwise to a solution of sodium metal in tetrahydrofuran (10 g of sodium metal and 1000 g of tetrahydrofuran), react at room temperature for 24 h, remove the solvent by rotary evaporation, and dry to obtain magnolol sodium;
[0083] Weigh 25 g of the prepared sodium magnololate, add it to 500 g of a tetrahydrofuran solution of polydichlorophosphazene (50 g of polydichlorophosphazene, 450 g of tetrahydrofuran), react at 120° C. for 10 h, cool, remove the solvent by rotary evaporation, and dry to obtain a 5',5-diallyl-2,2'-biphenyldioxy substituted polyphosphazene derivative.
[0084] The method for modifying phenolic fiber using the above composition comprises the following steps:
[0085] Step a, weighing each component according to the designed ratio of the above-mentioned composition, and mixing the weighed components uniformly to obtain a modified solution;
[0086] Step b, immersing the phenolic fiber in the modified solution at room temperature, with a bath ratio of 1:10, an immersion time of 5 minutes, drying at 75° C. to constant weight, and chopping the phenolic fiber, with the length of the chopped fiber being 6 mm, to obtain polyphosphazene modified phenolic fiber.
[0087] This embodiment also provides a flexible thermal insulation material, comprising the following raw material components in parts by weight: 85 parts of polyphosphazene, 9 parts of zinc oxide, 20 parts of white carbon black, 10 parts of phenolic resin, 8 parts of diisopropylbenzene peroxide and 10 parts of the polyphosphazene modified phenolic fiber prepared above.
[0088] The preparation method of the above-mentioned flexible thermal insulation material comprises the following steps:
[0089] Weigh each component according to the above ratio, add each component into an open mill, mix at 25°C, mix evenly, thin out a sheet, and hot press vulcanize. The hot press vulcanization temperature is 180°C, the pressure is 2MPa, and the time is t 100 min, to obtain the flexible thermal insulation material.
[0090] The flexible thermal insulation material prepared in this embodiment has a tensile strength of 15.3 MPa, an elongation at break of 256%, a linear ablation rate of 0.010 mm / s, and a mass ablation rate of 0.017 g / s.
[0091] Example 4
[0092] The embodiment of the present invention provides a composition for modifying phenolic fiber, comprising the following raw material components in parts by weight: 85 parts of ethoxy-substituted polyphosphazene derivative, 10 parts of white carbon black, 4 parts of zinc oxide, 3 parts of stearic acid, 4 parts of dicumyl peroxide and 140 parts of anhydrous ethanol.
[0093] The preparation method of the above-mentioned ethoxy-substituted polyphosphazene derivative comprises the following steps:
[0094] Weigh 50g of anhydrous ethanol and add it dropwise to a solution of sodium metal in tetrahydrofuran (10g of sodium metal and 1000g of tetrahydrofuran), react at room temperature for 24h, remove the solvent by rotary evaporation, and dry to obtain sodium ethoxide;
[0095] Weigh 25 g of the sodium ethoxide prepared above, add it to 500 g of a tetrahydrofuran solution of polydichlorophosphazene (50 g of polydichlorophosphazene, 450 g of tetrahydrofuran), react at 120° C. for 10 h, cool, remove the solvent by rotary evaporation, and dry to obtain an ethoxy-substituted polyphosphazene derivative.
[0096] The method for modifying phenolic fiber using the above composition comprises the following steps:
[0097] Step a, weighing each component according to the designed ratio of the above-mentioned composition, and mixing the weighed components uniformly to obtain a modified solution;
[0098] Step b, immersing the phenolic fiber in the modified solution at room temperature, with a bath ratio of 1:30, an immersion time of 4 minutes, drying at 75° C. to constant weight, and chopping the phenolic fiber, with the length of the chopped fiber being 9 mm, to obtain polyphosphazene modified phenolic fiber.
[0099] This embodiment also provides a flexible thermal insulation material, comprising the following raw material components in parts by weight: 80 parts of silicone elastomer, 1 part of zinc oxide, 60 parts of white carbon black, 20 parts of phenolic resin, 1 part of diisopropylbenzene peroxide and 70 parts of the polyphosphazene modified phenolic fiber prepared above.
[0100] The preparation method of the above-mentioned flexible thermal insulation material comprises the following steps:
[0101] Weigh each component according to the above ratio, add each component into an open mill, mix at 40°C, mix evenly, thin out a sheet, and hot press vulcanize. The hot press vulcanization temperature is 160°C, the pressure is 5MPa, and the time is t 90 min, to obtain the flexible thermal insulation material.
[0102] The flexible thermal insulation material prepared in this embodiment has a tensile strength of 6.7 MPa, an elongation at break of 175%, a linear ablation rate of 0.030 mm / s, and a mass ablation rate of 0.023 g / s.
[0103] Example 5
[0104] The embodiment of the present invention provides a composition for modifying phenolic fiber, comprising the following raw material components in parts by weight: 80 parts of a phenoxy-substituted polyphosphazene derivative, 20 parts of white carbon black, 6 parts of zinc oxide, 1 part of stearic acid, 3 parts of dicumyl peroxide and 100 parts of dioxane.
[0105] The preparation method of the above-mentioned phenoxy substituted polyphosphazene derivative comprises the following steps:
[0106] Weigh 50 g of phenol and add it dropwise to a solution of sodium metal in tetrahydrofuran (10 g of sodium metal and 1000 g of tetrahydrofuran), react at room temperature for 24 h, remove the solvent by rotary evaporation, and dry to obtain sodium phenolate;
[0107] Weigh 25 g of the sodium phenolate prepared above, add it to 500 g of a tetrahydrofuran solution of polydichlorophosphazene (50 g of polydichlorophosphazene, 450 g of tetrahydrofuran), react at 120° C. for 10 h, cool, remove the solvent by rotary evaporation, and dry to obtain a phenoxy-substituted polyphosphazene derivative.
[0108] The method for modifying phenolic fiber using the above composition comprises the following steps:
[0109] Step a, weighing each component according to the designed ratio of the above-mentioned composition, and mixing the weighed components uniformly to obtain a modified solution;
[0110] Step b, immersing the phenolic fiber fabric in the modified solution at room temperature, with a bath ratio of 1:45, an immersion time of 8 minutes, and drying at 75° C. to constant weight to obtain polyphosphazene modified phenolic fiber.
[0111] This embodiment also provides a flexible thermal insulation material, comprising the following raw material components in parts by weight: 95 parts of polyphosphazene, 5 parts of zinc oxide, 30 parts of white carbon black, 30 parts of phenolic resin, 5 parts of diisopropylbenzene peroxide and 90 parts of the polyphosphazene modified phenolic fiber prepared above.
[0112] The preparation method of the above-mentioned flexible thermal insulation material comprises the following steps:
[0113] Weigh each component according to the above ratio, add the weighed polyphosphazene, zinc oxide, white carbon black, phenolic resin and dicumyl peroxide into an open mill, blend at 35° C., mix evenly, and thinly pass through to obtain a film;
[0114] The polyphosphazene modified phenolic fiber fabric was cut into the same size as the film, placed between the two films, cross-stacked into a sandwich structure, placed in a mold, and then hot-pressed and vulcanized. The hot-pressing and vulcanization temperature was 165°C, the pressure was 5 MPa, and the time was t 90 min, to obtain the flexible thermal insulation material.
[0115] The flexible thermal insulation material prepared in this embodiment has a tensile strength of 35.1 MPa, an elongation at break of 58%, a linear ablation rate of 0.003 mm / s, and a mass ablation rate of 0.009 g / s.
[0116] Comparative Example 1
[0117] This comparative example provides a flexible thermal insulation material, the preparation method is the same as that of Example 5, except that the phenolic fiber is not modified. The flexible thermal insulation material includes the following raw material components in parts by weight:
[0118] 95 parts of polyphosphazene, 5 parts of zinc oxide, 30 parts of white carbon black, 30 parts of phenolic resin, 5 parts of dicumyl peroxide and 90 parts of phenolic fiber.
[0119] The preparation method of the above-mentioned flexible thermal insulation material comprises the following steps:
[0120] Weigh each component according to the above ratio, add the weighed polyphosphazene, zinc oxide, white carbon black, phenolic resin and dicumyl peroxide into an open mill, blend at 35° C., mix evenly, and thinly pass through to obtain a film;
[0121] After the phenolic fiber fabric is cut into the same size as the film, it is placed between the two films, cross-stacked into a sandwich structure and placed in a mold, and then hot-pressed and vulcanized. The hot-pressing and vulcanization temperature is 165°C, the pressure is 5MPa, and the time is t 90 min, to obtain the flexible thermal insulation material.
[0122] The flexible thermal insulation material prepared in this embodiment has a tensile strength of 17.5 MPa, an elongation at break of 25%, a linear ablation rate of 0.124 mm / s, and a mass ablation rate of 0.131 g / s.
[0123] Comparative Example 2
[0124] This comparative example provides a flexible thermal insulation material, and its preparation method is the same as that of Example 5, except that anthraquinone is used to replace polyphosphazene to modify the phenolic fiber. The composition for modifying the phenolic fiber includes the following raw material components in parts by weight: 80 parts of anthraquinone substituted polyphosphazene derivative, 20 parts of white carbon black, 6 parts of zinc oxide, 1 part of stearic acid, 3 parts of diisopropylbenzene peroxide and 100 parts of dioxane.
[0125] The preparation method of anthracenol substituted polyphosphazene derivative comprises the following steps:
[0126] Weigh 50g of anthracenol and add dropwise to a solution of sodium metal in tetrahydrofuran (10g of sodium metal and 1000g of tetrahydrofuran), react at room temperature for 36h, remove the solvent by rotary evaporation, and dry to obtain a sodium salt;
[0127] Weigh 25 g of the sodium salt prepared above, add it to 500 g of a tetrahydrofuran solution of polydichlorophosphazene (50 g of polydichlorophosphazene, 450 g of tetrahydrofuran), react at 120° C. for 4 h, cool, remove the solvent by rotary evaporation, and dry to obtain anthracene substituted polyphosphazene.
[0128] Then, the above-mentioned anthraphenol was used to replace the polyphosphazene to prepare a flexible thermal insulation material according to the same formula and method as in Example 5.
[0129] The flexible thermal insulation material prepared in this embodiment has a tensile strength of 5.4 MPa, an elongation at break of 27%, a linear ablation rate of 0.092 mm / s, and a mass ablation rate of 0.071 g / s.
[0130] The other aryloxy or alkoxy substituted polyphosphazenes described in the present invention can be prepared according to the above method, and the specific reaction conditions can be adjusted routinely by those skilled in the art.
[0131] The activator, reinforcing agent, heat-resistant filler and vulcanization aid in the above embodiments 1-5 can all be other components or a combination of multiple components defined in the present invention. There is no specific requirement for the ratio between the components in the composition, which can be adjusted by conventional tests. As long as the added amount is within the dosage range defined in the present invention, the technical effect basically equivalent to that of the corresponding embodiment can be achieved.
[0132] Similarly, by replacing the polyphosphazene derivatives in the above embodiments 1-5 with other aryloxy or alkoxy substituted polyphosphazene derivatives defined in the present invention, as long as the added amount is within the dosage range defined in the present invention, the technical effects substantially equivalent to those of the corresponding embodiments can be achieved.
[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A composition for modifying phenolic fiber, characterized in that: The invention comprises the following components in parts by weight: 80-100 parts of a polyphosphazene derivative, 10-60 parts of a reinforcing agent, 1-10 parts of an activator, 1-10 parts of a plasticizer, 1-10 parts of a vulcanizing agent and 100-200 parts of an organic solvent; Wherein, the polyphosphazene derivative is a polyphosphazene substituted with an alkoxy group and / or an aryloxy group; The aryloxy group is phenoxy, 4-ethylphenoxy, 2-methoxy-4-(2-propenyl)phenoxy, 4-propenyl-2-methoxyphenoxy, 2-allylphenoxy, 5',5-diallyl-2,2'-biphenyldioxy or 4-allyl-2,6-dimethoxyphenoxy; The alkoxy group is ethoxy, trifluoroethoxy or octafluoropentyloxy.
2. The composition for modifying phenolic fiber according to claim 1, characterized in that: The preparation method of the polyphosphazene derivative comprises: adding aromatic phenol and / or organic alcohol dropwise to a tetrahydrofuran solution of metallic sodium, reacting at 20° C.-40° C. for 6 h-24 h to obtain an organic sodium salt; Adding the organic sodium salt to a tetrahydrofuran solution of polydichlorophosphazene, reacting at 115° C.-125° C. for 6 h-24 h, removing the solvent, and drying to obtain the polyphosphazene derivative; The aromatic phenol is phenol, 4-ethylphenol, eugenol, isoeugenol, 2-allylphenol, magnolol or 4-allyl-2,6-dimethoxyphenol; the organic alcohol is ethanol, trifluoroethanol or octafluoropentanol.
3. The composition for modifying phenolic fiber according to claim 1 or 2, characterized in that: The reinforcing agent is white carbon black; and / or The activator is zinc oxide; and / or The plasticizer is stearic acid; and / or The vulcanizing agent is dicumyl peroxide; and / or The organic solvent is at least one of tetrahydrofuran, xylene, acetone, ethanol or dioxane.
4. A polyphosphazene-modified phenolic fiber, characterized in that: The phenolic fiber is obtained by modifying the composition according to any one of claims 1 to 3.
5. The method for preparing the polyphosphazene-modified phenolic fiber according to claim 4, characterized in that: The steps include: Step a, weighing each component according to the designed ratio of the composition according to any one of claims 1 to 3, and mixing the weighed components uniformly to obtain a modified solution; Step b, impregnating the phenolic fiber or phenolic fiber fabric with the modification solution, and drying to obtain polyphosphazene modified phenolic fiber.
6. A flexible thermal insulation material, characterized in that: The invention comprises the following raw material components in parts by weight: 80-100 parts of a heat insulating material matrix, 1-10 parts of an activator, 20-60 parts of a reinforcing agent, 10-60 parts of a heat-resistant filler, 1-10 parts of a vulcanizing aid and 5-90 parts of the polyphosphazene-modified phenolic fiber according to claim 4.
7. The flexible thermal insulation material according to claim 6, characterized in that: The thermal insulation material matrix is at least one of polyphosphazene rubber, EPDM rubber, nitrile rubber or silicone rubber; and / or The activator is at least one of zinc oxide, magnesium oxide, zinc methacrylate, zinc stearate or magnesium stearate; and / or The reinforcing agent is at least one of white carbon black, carbon black or modified white carbon black; and / or The heat-resistant filler is at least one of silicon dioxide, phenolic resin, epoxy resin, silicon carbide, aluminum oxide, antimony trioxide, boric acid, zinc borate, aluminum hydroxide or boron nitride.
8. The flexible thermal insulation material according to claim 6, characterized in that: The vulcanization aid includes at least one of sulfur, dicumyl peroxide or benzoyl peroxide.
9. A method for preparing the flexible thermal insulation material according to any one of claims 6 to 8, characterized in that: The steps include: The components are weighed according to the designed proportions, compounded, hot-pressed and vulcanized to obtain the flexible thermal insulation material.
10. The method for preparing the flexible thermal insulation material according to claim 9, characterized in that: If the polyphosphazene-modified phenolic fiber is a short fiber, the weighed components are added into an open mill for blending, the blending is uniform, a thin sheet is produced, and hot-pressed and vulcanized to obtain the flexible thermal insulation material; If the polyphosphazene-modified phenolic fiber is a fiber fabric, the weighed insulation material matrix, activator, reinforcing agent, heat-resistant filler and vulcanization aid are added to an open mill for blending, and the mixing is uniform and thinned out to obtain a film; after the polyphosphazene-modified phenolic fiber is cut into the same size as the film, it is placed between two films, hot-pressed and vulcanized to obtain the flexible insulation material.