A method for preparing oxide-modified ternary positive electrode material

By forming a hollow spherical metal oxide cladding layer on the surface of the ternary positive electrode material, the problem of insufficient cycling and rate performance of the high-Ni ternary positive electrode material is solved, and the electrochemical performance and cost reduction of the material are improved.

CN115881923BActive Publication Date: 2024-12-03HUADING GUOLIAN BATTERY MATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202211737481.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-31
Publication Date
2024-12-03
Estimated Expiration
2042-12-31

AI Technical Summary

Technical Problem

High Ni ternary cathode materials have shortcomings in circulation and rate performance, and their surface structure is unstable, which is easy to react with the electrolyte, resulting in a decrease in electrochemical performance.

Method used

The carbon template method assisted by hydrothermal method/solvent thermal method is used to prepare hollow spherical metal oxides and coat them on the surface of the ternary positive electrode material to form a uniform conductive network coating layer, and optimize the coating amount and conditions through mechanical ball mill mixing. , improve the structural stability and electrochemical properties of the material.

Benefits of technology

It effectively suppresses the side reaction between the ternary positive electrode material and the electrolyte, improves the cyclic stability and rate performance of the material, enhances the electrochemical performance, reduces costs and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115881923B_ABST
    Figure CN115881923B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing an oxide-modified ternary cathode material, comprising the following steps: preparing a metal oxide having a hollow sphere structure by using a carbon template method to assist a hydrothermal method / solvothermal method; mixing a ternary precursor with a lithium source and calcining the mixture to obtain a ternary cathode calcined product; mixing the metal oxide and the ternary cathode calcined product and calcining the mixture again to obtain a ternary cathode material coated with a hollow sphere. The technical solution provided by the present invention is simple and is conducive to cost reduction compared with the same type of liquid phase method. By forming a uniform coating layer on the surface of the ternary cathode material, the side reaction between the ternary cathode material and the electrolyte can be effectively suppressed, thereby improving the rate performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery positive electrode material preparation, and in particular to a method for preparing a metal oxide modified ternary positive electrode material. Background Art

[0002] Ternary cathode materials (NCM) have attracted much attention due to their outstanding advantages such as high power density, energy density, and excellent cycle performance. In recent years, society has placed higher and higher demands on the specific energy of batteries, and ternary cathode materials can obtain higher specific capacity as the Ni content continues to increase. Therefore, high-Ni ternary cathode materials have become a research hotspot. Inevitably, there are some problems that need to be solved with high-Ni ternary cathode materials. They are mainly attributed to several aspects. One is that the cycle performance and rate performance deteriorate. This is because as the Ni content increases, Li + / Ni 2+ The cation mixing increases, and the quality of the active material is damaged during the cycle. Ion mixing will cause some nickel ions to be distributed in the lithium layer, thus affecting the transmission rate of lithium ions. 4+ The first is that the material structure stability decreases. Second, the residual lithium content on the surface of the high-Ni ternary positive electrode material increases. The residual lithium easily reacts with the lithium salt in the electrolyte. Third, the surface structure of the particles is unstable. More Li is required to participate in ion transport during the charge and discharge process. This causes irreversible damage to the layered ternary positive electrode material and even causes structural collapse. At this time, a more stable crystal structure is needed to meet the high capacity requirements.

[0003] In response to the above problems, the main modification methods include optimizing material preparation process, ion doping and surface coating. At present, the industry mostly uses high-temperature solid-phase method to prepare ternary positive electrode materials. In the process of generating finished ternary positive electrode materials by high-temperature solid-phase method, factors such as lithium content, sintering system, oxygen flow rate, etc. can affect the intrinsic properties of the material. Adjusting the process parameters can obtain better morphology, tap density and particle size distribution. In short, the individual composition, structure and morphology modification of the ternary positive electrode material will affect the electrochemical properties of the positive electrode material. Among the many modification methods, the bulk doping modification method is one of the most common modification methods because of its easy control and obvious effect. Cation doping can enhance the structural stability of the ternary positive electrode material and reduce Li + / Ni 2+Cation mixing. In addition, surface coating with oxides, lithium ion conductors or phosphates can prevent direct contact between the material and the electrolyte, isolate the corrosion of the electrolyte on the positive electrode material, and improve the interface stability of the material. However, the effect of a single modification is still not ideal, so synergistic modification is currently a research direction favored by researchers. At present, the most commonly used synergistic modification methods are double / multi-ion synergistic doping, and a combination of doping and coating. Theoretically, the physicochemical properties of the coating material are also affected by the structure and composition. Therefore, this patent proposes a new synergistic modification method, which first optimizes the physicochemical properties of the coating material by adjusting the structure of the coating material, and then composites the structurally modified coating material with the ternary positive electrode material to improve the electrochemical properties of the ternary positive electrode material.

[0004] CN202210729961 provides a method for preparing a MXene-coated ternary cathode material, comprising the following steps: firstly, MXene is prepared by etching, then a ternary precursor and a lithium source are mixed, and calcined once to obtain a ternary cathode calcined product, and then a dispersant, MXene and the ternary cathode calcined product are mixed, and calcined twice to obtain a MXene-coated ternary cathode material. The electrochemical properties of the ternary cathode material, such as rate performance, high temperature cycle and high temperature storage, are improved.

[0005] CN109599537A proposes a method for preparing xBiPO4 / (1-x)BiOBr coating materials by a liquid phase method, and then coating xBiPO4 / (1-x)BiOBr on the surface of a ternary positive electrode material by a solid phase method. The coating material preparation process is briefly described as follows: Bi(NO3)3·5H2O is dissolved in a mixed solution of deionized water and anhydrous acetic acid to obtain a mixed solution A. Na2HPO4·12H2O and KBr are dissolved in deionized water to obtain a mixed solution B. Solution B is slowly added dropwise to mixed solution A to obtain a suspension, which is then transferred to a reactor to react at 120℃-220℃ for 5-20h, followed by centrifugation, water washing, and drying to obtain a coating material. The solid phase coating ternary positive electrode material preparation process is briefly described as follows: The ternary positive electrode material Li 1+a Ni 1-b-c Co b Mn c O2 (0≤a≤0.15, 0.1≤b+c≤0.4) powder and xBiPO4 / (1-x)BiOBr were ball-milled in a dry atmosphere to obtain the coated lithium-ion battery composite cathode material precursor powder xBiPO4 / (1-x)BiOBr@Li 1+a Ni 1-b-c Co b Mn cO2. After high-temperature sintering in a muffle furnace, a composite positive electrode material for lithium-ion batteries was obtained, which improved the electrochemical performance of the ternary positive electrode material.

[0006] In the above technical solutions, the ternary cathode material is coated and modified, but CN202210729961 mixes MXene with the ternary cathode material to form a composite material. Because the combination of MXene and the ternary cathode material is prone to MXene detaching from the main body of the ternary cathode material, a dispersant needs to be added, resulting in increased costs. CN109599537A uses a slow dripping mixing method, which is time-consuming and not conducive to industrial mass production. Therefore, how to optimize and improve the preparation process of the material and provide a ternary cathode material composite with a structurally modified coating material is a problem that needs to be solved in the field of lithium-ion battery cathode material preparation technology. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a method for preparing an oxide-modified ternary positive electrode material, which regulates the structure of the coating material, prepares a metal oxide with a hollow morphology and coats the metal oxide on the surface of the ternary positive electrode material, thereby forming a uniform conductive network coating layer on the surface of the ternary positive electrode material, which can effectively inhibit the side reaction between the ternary positive electrode material and the electrolyte, thereby improving the electrochemical properties of the material.

[0008] A method for preparing an oxide-modified ternary positive electrode material comprises the following steps:

[0009] s1. Use carbon template method to assist hydrothermal method / solvothermal method to prepare metal oxides with hollow sphere structure.

[0010] s2. Mix the ternary precursor and the lithium source and calcine them to obtain a ternary positive electrode product.

[0011] s3. The metal oxide prepared in step s1 and the ternary positive electrode sintered product obtained in step s2 are mixed and calcined again to obtain a ternary positive electrode material coated with hollow spheres.

[0012] Although ternary cathode materials have obvious advantages in lithium-ion batteries, they also have shortcomings, such as rapid battery capacity decay and poor rate performance at high current density. Studies have shown that the capacity decay of cathode active materials is closely related to the physical and chemical properties of the material particle surface, because Li + The diffusion migration and interfacial charge transfer of Li+ need to pass through the material surface. Many research reports have also confirmed that the surface coating modification method can reduce the side reaction between the electrolyte and the electrode material, ensuring the Li+ +The main structure is stable during the long cycle insertion / extraction process, resulting in excellent electrochemical performance. Common coatings include metal oxides (Al2O3, ZrO2, CeO2, TiO2, MgO), fluorides (LiF), phosphates (Li3PO4), etc.

[0013] Since the effect of coating methods on the performance of ternary cathode materials is highly dependent on the performance, content, heat treatment conditions, etc. of the coating materials. Therefore, regulating the structure of the coating material is beneficial to improving the electrochemical performance of high-Ni ternary cathode materials. Hollow microspheres have both relatively large interface advantages and relatively stable material structures, which effectively ensure the cyclic stability of the material. The template method is divided into hard template method and soft template method. Removing hard templates often requires strong acids and strong bases, while the removal of soft templates only requires high-temperature calcination, so it is more environmentally friendly and economical.

[0014] Furthermore, step s1 includes s11 and s12, which are specifically as follows.

[0015] s11. Preparation of carbon sphere template

[0016] The carbon source and the solvent are mixed to prepare a solution, a precipitate is obtained by a hydrothermal method or a solvothermal method, and the precipitate is washed and dried to obtain a carbon sphere template.

[0017] The carbon source may be any one of starch, fructose, sucrose, and glucose; the solvent may be water or a mixed solution of water and ethanol, such as a mixed solution of water and ethanol in a volume ratio of 1:1;

[0018] In this step, the hydrothermal / solvothermal heating temperature is 160-180°C, and the insulation time is 14-18h.

[0019] s12. Preparation of metal oxides with hollow sphere structures

[0020] According to the desired metal oxide, a metal source, the carbon sphere template in step s11 and a solvent are mixed to prepare a solution, a precipitate is obtained by a solvothermal method, and the precipitate is calcined to obtain a metal oxide with a hollow sphere structure.

[0021] The metal oxide described in the present invention is preferably indium oxide, zinc oxide, titanium oxide or tungsten oxide. A series of hollow metal oxide materials can be prepared by regulating the hydrothermal / solvothermal conditions (temperature, time, pH).

[0022] Among them, indium oxide (In2O3) is a wide-gap semiconductor with good electrical conductivity and a body-centered cubic crystal structure. Its good stability makes it widely used in solar cells, electronics and other fields. In2O3 is used as a coating material to obtain excellent electrochemical performance. The present invention adopts a soft template method to assist the solvothermal method to prepare In2O3 hollow microspheres with uniform size distribution, and the hollow In2O3 is coated on the ternary positive electrode material to slow down the side reaction between the ternary positive electrode material and the electrolyte, alleviate the phase change of H2-H3, and improve the cycle stability and rate performance of the ternary positive electrode material.

[0023] In step s12, the solvent can be water, a mixed solution of water and ethanol in any ratio, or a mixed solution of water and an organic solvent; wherein the organic solvent can be at least one of ethanol, PEG200 or PEG2000; for example, a 1:1 mixed solution of water and ethanol, or a mixed solution of water, ethanol, PEG200, etc.

[0024] In step s12, the solvent heating temperature ranges from 150 to 180°C, and the insulation time ranges from 20 to 24 hours.

[0025] In step s12, in order to ensure effective growth and development of the grains and avoid insufficient grain growth due to insufficient temperature and time, or excessive grain growth due to excessive temperature and time, the calcination temperature is 400-500°C and the holding time is 2-4h.

[0026] In step s12, a corresponding metal nitrate may be selected as a metal source. For example, if the metal oxide is indium oxide, indium nitrate is used as an indium source.

[0027] Step s2 of the present invention is: calcining the ternary precursor after mixing with a lithium source to obtain a ternary positive electrode product. Specifically, the material proportion of Ni in the ternary precursor includes any one of Ni80, Ni90 or Ni99. In the present invention, Ni80 means that the molar percentage content of Ni in the ternary precursor is 80%, and the same applies to Ni90 and Ni99. The calcination temperature in this step is 830-910°C, the holding time is 12-24h, and the calcination atmosphere is oxygen.

[0028] Step s3 of the present invention is: the metal oxide prepared in step s1 and the ternary positive electrode one sintered product obtained in step s2 are mixed and calcined again to obtain a ternary positive electrode material coated with a hollow sphere. Wherein, the mass fraction ratio of the metal oxide to the ternary positive electrode one sintered product is 0.1%-10%. If the coating amount is too high, the material coating layer will be too thick, which is not conducive to improving the material performance, and it is easy to form a dense coating, which is not conducive to ion diffusion, and it is easy to form an uneven coating, increasing material defects; while the coating amount is too low. The effect on material performance is small, so it is preferred that the mass fraction ratio of the metal oxide to the ternary positive electrode one sintered product is 0.1%-10%. The mixing method of the two is mechanical ball milling, the rotation speed is 400r / min, and the ball milling time is 30-50min. The calcination temperature in this step is 450-550℃, the insulation time is 5-12h, and the calcination atmosphere is oxygen.

[0029] The present invention regulates the structure of the coating material, synthesizes a carbon template with uniform morphology by a simple hydrothermal method, and further adjusts the structure of the coating material by a hydrothermal method to prepare In2O3 with a hollow morphology. Finally, by coating In2O3 on the surface of the ternary positive electrode material, a uniform conductive network coating layer is formed on the surface of the ternary positive electrode material, which can effectively inhibit the side reaction between the ternary positive electrode material and the electrolyte, thereby improving the electrochemical performance of the material. The prepared material has the advantages of high cycle retention rate and good rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The above and other features, advantages and aspects of the embodiments of the present application will become more apparent with reference to the following detailed description in conjunction with the accompanying drawings. In the accompanying drawings, the same or similar reference numerals represent the same or similar elements, wherein:

[0031] Figure 1 . Flow chart of the preparation process of carbon template assisted solvothermal method.

[0032] Figure 2 .Process flow chart for the preparation of high-Ni ternary positive electrode materials.

[0033] Figure 3 .Process flow chart for coating ternary positive electrode materials.

[0034] Figure 4 .First charge and discharge curve.

[0035] Figure 5 .Rate performance curve.

[0036] Figure 6 .The 100-day cycle curve of Example 2. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.

[0038] Example 1

[0039] This embodiment provides a method for hollow In2O3 coated high Ni ternary positive electrode material, which is prepared by the following steps:

[0040] (1) Preparation of carbon sphere template. Dissolve 5 g of glucose in 100 ml of deionized water to prepare a sugar solution of a certain concentration. Place the solution in a Teflon-lined stainless steel autoclave and keep it at 160°C for 10 hours. Then collect the precipitate by centrifugation, wash it several times with distilled water and ethanol, and finally dry it in an oven at 80°C for 12 hours to obtain a carbon sphere template with uniform morphology.

[0041] (2) Preparation of hollow In2O3. The carbon sphere template prepared in step (1) was dissolved in 100 ml of deionized water, ultrasonically shaken for 15 min, and then indium nitrate was added. After sufficient stirring and dissolution, the solution was transferred to a reactor, hydrothermally heated at 180°C for 24 h, and then centrifuged to collect the precipitate. The obtained precipitate was dried in an oven at 80°C for 12 h and then calcined at 450°C for 2 h to obtain hollow In2O3.

[0042] (3) Calcination. Weigh LiOH and NCM precursor according to the ratio of n(Li):n(Ni+Co+Mn)=1.08:1.00, mix them, ball mill at 400r / min for 30min, put them into a sagger, and place them in a muffle furnace (oxygen atmosphere). Heat to 850℃ at a rate of 2℃ / min and keep it warm for 20h. Crush the material and sieve it through 300 mesh to obtain the calcined product.

[0043] (4) Coating. The positive electrode material and the hollow In2O3 material were weighed according to a mass fraction ratio of 0.3%, and mixed in a ball mill at a speed of 200r / min for 50min. Then, the material was placed in a muffle furnace and kept at 480℃ for 8h under an oxygen atmosphere to obtain a hollow In2O3-coated high-Ni ternary positive electrode material.

[0044] Example 2

[0045] This embodiment provides a method for hollow In2O3 coated with high Ni ternary positive electrode material, which is prepared by the following steps: except that the mass fraction ratio of the positive electrode material to the hollow In2O3 material in step (4) is 0.5%, the remaining process steps are the same as those in Example 1.

[0046] Example 3

[0047] This embodiment provides a method for hollow In2O3 coated with high Ni ternary positive electrode material, which is prepared by the following steps: except that the mass fraction ratio of the positive electrode material to the hollow In2O3 material in step (4) is 0.7%, the remaining process steps are the same as Example 1.

[0048] Example 4

[0049] This embodiment provides a method for hollow In2O3 coated high Ni ternary positive electrode material, which is prepared by the following steps:

[0050] (1) Preparation of carbon sphere template. Dissolve 3 g of sucrose in 100 ml of a 1:1 mixed solution of deionized water and ethanol to prepare a sugar solution. Place the solution in a reactor and keep it at 180°C for 15 hours. Then collect the precipitate by centrifugation, wash it with distilled water and ethanol three times each, and finally dry it in an oven at 80°C to obtain a carbon sphere template with uniform morphology.

[0051] (2) Preparation of hollow In2O3. The carbon sphere template prepared in step (1) was dissolved in a mixed solution of 40 ml water, 40 ml ethanol and 20 ml PEG200, and indium nitrate was added after ultrasonic treatment for 15 min. After being fully dissolved, it was transferred to a reactor, kept at 150°C for 18 h, and then centrifuged and dried.

[0052] (3) Calcination: The calcination conditions are the same as those in Example 1 except that the temperature is 900° C. and the temperature is maintained for 15 h.

[0053] (4) Coating. Weigh the positive electrode material and the hollow In2O3 material in a ratio of 1% (mass fraction), mix at 200r / min, and mix for 30min. Then place the material in a muffle furnace and keep it at 470℃ in an oxygen atmosphere for 10h to obtain a hollow In2O3-coated high-Ni ternary positive electrode material.

[0054] Example 5

[0055] This embodiment provides a method for hollow In2O3 coated with high Ni ternary positive electrode material, which is prepared by the following steps: except that the mass fraction ratio of the positive electrode material to the hollow In2O3 material in step (4) is 5%, the remaining process steps are the same as Example 4.

[0056] Example 6

[0057] This embodiment provides a method for hollow In2O3 coated with high Ni ternary positive electrode material, which is prepared by the following steps: except that the mass fraction ratio of the positive electrode material to the hollow In2O3 material in step (4) is 10%, the remaining process steps are the same as Example 4.

[0058] Example 7

[0059] The present embodiment provides a method for hollow In2O3-coated high-Ni ternary positive electrode material, which is prepared by the following steps: except that the solution in step (2) is a mixed solution of 50 ml water, 15 ml ethanol, 15 ml PEG200, and 20 ml DMF, and the calcination condition in step (3) is a temperature of 900°C for 17 hours, the remaining process steps are the same as those in Example 1.

[0060] Comparative Example 1

[0061] This comparative example provides a method for preparing a ternary positive electrode material, and the preparation method is completely consistent with step (2) in Example 1.

[0062] The above-mentioned In2O3-coated ternary cathode material was made into a button half-cell for electrochemical performance testing. Test method: The voltage range was 3-4.3V, and the rate was 0.1C for specific capacity testing; the rate energy was tested under 0.1C, 0.2C, 0.5C, 1C, 3C, and 0.1C conditions. The improvement data results of each test content are shown in Table 1.

[0063] Table 1 Electrochemical performance data statistics

[0064]

[0065]

[0066] From Table 1 and Appendix Figure 4-6 The following conclusions can be drawn:

[0067] (1) It can be seen from Comparative Example 1 and Examples 2, 4, and 7 that the preparation method of the In2O3-coated ternary positive electrode material provided by the present invention can effectively inhibit the side reaction between the ternary positive electrode material and the electrolyte, improve the rate performance, and have good cycle performance.

[0068] (2) It can be seen from Examples 1-3 and Examples 4-6 that when the coating amount is different, the electrochemical performance improvement is different. When the carbon source changes, under the optimal conditions, the electrochemical performance of the material can still be improved.

[0069] (3) As can be seen from Example 7, the use of mixed solvents can still achieve the purpose of improving the electrochemical properties of the material. This example shows that it may help reduce costs in actual production.

[0070] (4) From Figure 6 It can be seen that the daytime cycle efficiency of Example 2 reaches 96.46%.

[0071] In summary, the preparation method of the modified In2O3-coated ternary positive electrode material provided by the present invention is simple and conducive to cost reduction (compared with the same type of liquid phase method). By forming a uniform coating layer on the surface of the ternary positive electrode material, the side reaction between the ternary positive electrode material and the electrolyte can be effectively inhibited, thereby improving the rate performance and cycle performance.

[0072] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing an oxide-modified ternary cathode material, characterized in that: The following steps are involved: s1. Using carbon template method to assist hydrothermal method / solvothermal method to prepare metal oxides with hollow sphere structure; s2, mixing the ternary precursor with the lithium source and calcining to obtain a ternary positive electrode product; s3, mixing the metal oxide prepared in step s1 and the ternary positive electrode sintered product obtained in step s2 and calcining them again, wherein the mass fraction ratio of the metal oxide to the ternary positive electrode sintered product is 0.1%-10%, to obtain a ternary positive electrode material coated with hollow spheres; Wherein, step s1 comprises the following steps: s11. Preparation of carbon sphere template The carbon source and the solvent are mixed to form a solution, a precipitate is obtained by a hydrothermal method or a solvothermal method, and the precipitate is washed and dried to obtain a carbon sphere template; s12. Preparation of metal oxides with hollow sphere structures According to the desired metal oxide, a metal source, the carbon sphere template in step s11 and a solvent are mixed to prepare a solution, a precipitate is obtained by a solvothermal method, and the precipitate is calcined to obtain a metal oxide with a hollow sphere structure.

2. The preparation method according to claim 1, characterized in that: The metal oxide is indium oxide, zinc oxide, titanium oxide or tungsten oxide.

3. The preparation method according to claim 1, characterized in that: In step s11, any one of starch, fructose, sucrose or glucose is used as the carbon source.

4. The preparation method according to claim 1, characterized in that: The solvent used in step s1 includes at least one of ethanol, PEG200 or PEG2000.

5. The preparation method according to claim 1, characterized in that: The heating temperature of the hydrothermal method or the solvent thermal method in step s11 is 160-180° C., and the insulation time is 14-18 hours.

6. The preparation method according to claim 1, characterized in that: The heating temperature of the solvothermal method in step s12 is 150-180° C., and the insulation time is 20-24 hours.

7. The preparation method according to claim 1, characterized in that: In step s2, the calcination temperature is 830-910° C. and the insulation time is 12-24 hours.

8. The preparation method according to claim 1, characterized in that: The calcination temperature in step s3 is 450-550° C., and the holding time is 5-12 hours.

Citation Information

Patent Citations

  • Lithium ion battery composite positive electrode material and preparation method thereof

    CN109599537A

  • MXene-coated ternary positive electrode material, preparation method thereof and lithium ion battery

    CN114883550A

  • Multi-shell metal oxide hollow sphere synthesized based on anion adsorption and preparation method as well as application thereof

    CN105762349A

  • Ternary anode material with metallic oxide coated surface and preparation method of ternary anode material

    CN108258224A

  • Nanoparticle-encapsulated multi-core multi-shell hollow material as well as preparation method and application thereof