A low temperature starting lithium ion battery and preparation method thereof

Through magnetic induction, the cathode material with a nickel-cobalt-manganese gradient dispersion and the graphene-coated negative electrode material with lithium titanate are formed. Combined with a modified electrolyte, the problem of difficult starting and capacity decay of lithium-ion batteries in low-temperature environments is solved, and the problem of lithium-ion batteries is difficult to start and attenuate in low-temperature environments is improved. Lithium ion diffusion rate and electron mobility extend the battery life and enhance cycling stability.

CN115881940BActive Publication Date: 2024-11-12JIANGNAN ELECTROMECHANICAL DESIGN INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211025555.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-25
Publication Date
2024-11-12
Estimated Expiration
2042-08-25

AI Technical Summary

Technical Problem

The existing low-temperature startup lithium-ion batteries increase charge and discharge impedance under long-term low-temperature and high-speed magnification conditions, decrease electrochemical performance, and insufficient ionic conductivity and compatibility of electrolyte solvents, resulting in difficulty in starting, fast capacity decay, and short battery life. The problem.

Method used

The lithium-rich manganese-based positive electrode material is used to induced magnetically to form a nickel-cobalt-manganese gradient dispersion, combined with graphene-coated negative electrode material of lithium titanate, and modified electrolyte solvent to improve the diffusion rate of lithium ion and electron mobility. Lithium-ion battery with excellent low-temperature starting performance.

Benefits of technology

It improves the lithium ion diffusion rate and electron mobility of lithium-ion batteries in low-temperature environments, extends the battery life, enhances the cycle stability and low-temperature rate performance, and overcomes the difficult start-up and capacity attenuation of the battery in low-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115881940B_ABST
    Figure CN115881940B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium ion batteries, and specifically relates to a low-temperature starting lithium ion battery and a preparation method thereof; in the present invention, the positive electrode adopts a high electrochemical performance positive electrode material formed by magnetic induction to form a nickel-cobalt-manganese gradient dispersion; the electrolyte solvent adopts ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate as the base solution, and adds propylene carbonate, ethylene carbonate and ethyl acetate antifreeze additives; the negative electrode adopts a graphene-coated "zero strain" lithium titanate composite material with high electron mobility. By combining the above-mentioned positive electrode, negative electrode and electrolyte solvent, a lithium ion battery with excellent low-temperature starting performance is formed, the lithium ion diffusion rate and electron mobility of lithium ions in a low-temperature environment are improved, and the problems of lithium ion batteries being difficult to start in a low-temperature environment, fast capacity decay, and short battery life are effectively overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a low-temperature starting lithium ion battery and a preparation method thereof. Background Art

[0002] Existing low-temperature starting lithium-ion batteries have the following technical difficulties: 1. Low electron mobility and lithium ion diffusion rate, which are decisive factors of the positive electrode material; 2. Ionic conductivity and compatibility of the electrolyte solvent; 3. Lithium insertion capacity and electron mobility of the negative electrode material.

[0003] The patent document with announcement number CN109286008A discloses a low-temperature lithium-ion battery and a preparation method thereof, which mainly improves the electrochemical performance of the lithium-ion battery by changing the ratio of the positive electrode sheet, the negative electrode sheet and the electrolyte. However, the traditional preparation method is difficult to change the atomic distribution of the structure of the positive electrode material itself, and there is a concentration gradient in the nickel, cobalt and manganese atoms, which leads to an increase in the charge and discharge impedance of the lithium-ion battery under long-term low temperature and high rate conditions, and a decrease in the electrochemical performance. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a low-temperature starting lithium ion battery and a preparation method thereof.

[0005] This is achieved specifically through the following technical solutions:

[0006] 1. A low-temperature starting lithium-ion battery, comprising a magnetically induced positive electrode material, an electrolyte and a negative electrode material;

[0007] Furthermore, the magnetically induced positive electrode material is a lithium-rich manganese-based positive electrode material with a nickel-cobalt-manganese gradient dispersion formed by dispersing a lithium source, a nickel source, a cobalt source and a manganese source in a solvent under magnetic induction conditions, and then calcining and cooling, wherein the molar ratio of the nickel source, the cobalt source and the manganese source is 0.13:0.13:0.54;

[0008] Furthermore, the electrolyte is prepared by using ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate as a basic solution, and then adding additives;

[0009] Furthermore, the negative electrode material is a composite material made of graphene coated lithium titanate.

[0010] Furthermore, the lithium source is at least one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium acetate dihydrate and lithium hydroxide monohydrate.

[0011] Furthermore, the nickel source is at least one of nickel acetate, nickel hydroxide, and nickel carbonate; the cobalt source is at least one of cobalt acetate, cobalt hydroxide, and cobalt carbonate; and the manganese source is at least one of manganese acetate, manganese hydroxide, and manganese carbonate.

[0012] Furthermore, the ratio of the amount of lithium contained in the lithium source to the total amount of Ni, Co, and Mn in the lithium-rich manganese-based precursor is 1.5-1.6: 1. For example, it can be 1.5: 1, 1.51: 1, 1.52: 1, 1.53: 1, 1.54: 1, 1.55: 1, 1.56: 1, 1.57: 1, 1.58: 1, 1.59: 1, 1.60: 1, and any value in the range formed by any two of these point values.

[0013] Furthermore, the additive accounts for 11-40% (v%) in the electrolyte; the volume addition ratio of the additive is propylene carbonate: ethylene carbonate; ethyl acetate = 1-10%: 0.5-5%: 10-25%.

[0014] Furthermore, the ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 2:3:5 (w / w / w).

[0015] Furthermore, the lithium salt is lithium hexafluorophosphate with a concentration of 1.2 mol / L.

[0016] 2. The preparation method of the magnetic induction positive electrode material of the low temperature starting lithium ion battery comprises the following steps:

[0017] (1) dispersing a lithium source, a nickel source, a cobalt source and a manganese source into a solvent, uniformly mixing them under a magnetic stirrer, evaporating them, and forming a mixed slurry under magnetic induction;

[0018] (2) The mixed slurry is subjected to secondary calcination and cooling to form a lithium-rich manganese-based positive electrode material.

[0019] Furthermore, the stirring conditions are: stirring speed of 100-2000rpm / min, stirring temperature of 20-100°C, stirring time of 1-10h; the evaporation conditions are: stirring speed of 100-2000rpm / min, evaporation temperature of 80-180°C, evaporation time of 8-24h.

[0020] Furthermore, the secondary calcination is performed twice in an air atmosphere, the first calcination is performed at a temperature of 350-500° C. for 4-6 hours, and the second calcination is performed at a temperature of 850-1000° C. for 10-15 hours.

[0021] 3. The negative electrode material of the low-temperature start lithium-ion battery, and the preparation method thereof comprises the following steps;

[0022] (1) adding a titanium source into a buffer solution and dispersing the solution by ultrasonication to form a mixed solution;

[0023] (2) adding a single-sheet graphene dispersion to the mixed dispersion, adding a lithium source after continuous ultrasonic dispersion at room temperature, and obtaining a composite after centrifugal washing;

[0024] (3) The composite is calcined at 600-1000° C. in an inert atmosphere for 8-24 hours, and then naturally cooled to obtain a graphene-coated lithium titanate composite material.

[0025] Furthermore, the titanium source is one or two of titanium dioxide and tetratinyl titanate; the buffer solution is one or more of ethanol, methanol or acetone.

[0026] Furthermore, the stirring conditions include: a stirring speed of 100-2000 rpm / min, a stirring temperature of 20-100° C., and a stirring time of 0.5-5 h.

[0027] Furthermore, the concentration of the single-sheet graphene dispersion is 5-10 mg / mL, and the mass ratio of the composite to the single-sheet graphene is 10-100:1.

[0028] Furthermore, the lithium source may be selected from at least one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium acetate dihydrate and lithium hydroxide monohydrate.

[0029] 4. Battery assembly: Take magnetically induced lithium-rich manganese-based positive electrode material, add conductive carbon black as a conductive agent and polyvinylidene fluoride as a binder to prepare positive electrode slurry; take graphene-coated lithium titanate material (negative electrode material), add conductive carbon black as a conductive agent and polyvinylidene fluoride as a binder to prepare negative electrode slurry; add electrolyte dropwise.

[0030] The prepared slurry is coated, then rolled, slit and die-cut. The compaction density of the positive electrode is 3.6 g / cm 3 The compaction density of the negative electrode roller is 1.65g / cm 3 The die-cut positive and negative electrode sheets are stacked, encapsulated with aluminum-plastic film once, dried, injected with liquid, formed, encapsulated with aluminum-plastic film twice, and divided into different capacities to prepare a soft-pack full battery.

[0031] In summary, the beneficial effects of the present invention are as follows: in the present invention, the positive electrode adopts a high electrochemical performance positive electrode material formed by magnetic induction to form a nickel-cobalt-manganese gradient dispersion; the electrolyte solvent adopts ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate as the base solution, and adds propylene carbonate, ethylene carbonate and ethyl acetate antifreeze additives; the negative electrode adopts a "zero strain" lithium titanate composite material coated with graphene with high electron mobility. By combining the above positive electrode, negative electrode and electrolyte solvent, a lithium ion battery with excellent low-temperature starting performance is formed, which improves the lithium ion diffusion rate and electron mobility of lithium ions in low-temperature environments, and effectively overcomes the problems of lithium ion batteries being difficult to start in low-temperature environments, fast capacity decay, and short battery life.

[0032] The present invention proposes for the first time that an external magnetic field is used to induce a lithium-rich manganese-based cathode material to form a nickel-cobalt-manganese dispersion layer with a gradient distribution, which is conducive to forming a stable interface structure and improving the cyclic stability of the material. This preparation forms a lithium-rich manganese-based cathode material by a hydrothermal method. Under the external force of a magnetic field, a driving force is provided for the transformation of the morphology and crystal structure, and its growth direction and structure are optimized, thereby obtaining a lithium-rich manganese-based cathode material with excellent electrochemical properties. In addition, the special ordered arrangement of Li / TM ions is conducive to the deintercalation of lithium ions and enhances its rate performance at low temperatures.

[0033] The traditional basic electrolyte solvent is composed of organic solvents such as ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). At low temperatures, the conductivity of the electrolyte will drop sharply, and it will even solidify and stratify to form a colloid. Based on the current problems, low co-solvent propylene carbonate, ethylene carbonate to reduce the initial lithium insertion decomposition of the negative electrode, and ethyl acetate to improve low-temperature conductivity are added to the above ratio to form a low-temperature composite electrolyte solvent with high performance.

[0034] The present invention uses lithium titanate, which has many advantages such as high safety, high power density, good low temperature performance, long life and small volume change. The "zero strain" characteristic helps to solve the safety hazards of lithium-ion batteries. At the same time, the two-dimensional honeycomb six-membered ring single graphite layer structure of graphene is used to improve its conductivity, excellent conductivity and ultra-large specific surface area.

[0035] In the above, the modified positive electrode, electrolyte and negative electrode together form a lithium-ion battery with high and low temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The soft-pack full batteries prepared in Example 1 and Comparative Examples 1-3 are within the voltage range of 2.0 to 4.8 V, 1 C (250 mAh g -1 ) Comparison of discharge specific capacity at different rates. DETAILED DESCRIPTION

[0037] The specific embodiments of the present invention are further described in detail below, but the present invention is not limited to these embodiments, and any improvement or substitution based on the basic spirit of the present embodiment still falls within the scope of protection required by the claims of the present invention. Example

[0038] The preparation method of a magnetically induced low-temperature starting lithium-ion battery comprises the following steps:

[0039] (1) Preparation of lithium-rich manganese-based positive electrode materials: nickel acetate, cobalt acetate and manganese acetate were added to 100 ml of distilled water according to a molar ratio of 0.13:0.13:0.54, and mixed evenly for 30 minutes at 50°C, 500 rpm / min, and a magnetic stirrer with a magnetic stirring of 1000w; lithium hydroxide was added according to the lithium source: (nickel source + cobalt source + manganese source) = 1.5:1, and mixed evenly for 30 minutes at 50°C, 500 rpm / min, and a magnetic stirrer with a magnetic stirring of 1000w; then evaporated at 110°C to form a mixed slurry. In an air atmosphere, the slurry was placed in a muffle furnace for calcination at a temperature of 500°C for 5 hours and at 900°C for 12 hours.

[0040] (2) Preparation of graphene-coated lithium titanate composite material (negative electrode material): 5g of titanium dioxide was added to 500ml of ethanol and dispersed at 25°C and 100rpm / min for 30min; then 10ml of a 10mg / mL single-layer graphene mixed solution was slowly added; finally, 1.9g of lithium carbonate was added and evaporated at 85°C and 100rpm / min to a slurry. Under an argon atmosphere, the temperature was 800°C and the calcination time was 10h to obtain a graphene-coated lithium titanate composite material.

[0041] (3) Preparation of low-temperature electrolyte: the solute is 1.2 mol / L lithium hexafluorophosphate; the solvent is ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a ratio of 2:3:5 (w / w / w); the solute accounts for 25% of the solvent by mass percentage; the mass ratio of electrolyte additives propylene carbonate: ethylene carbonate: ethyl acetate is 5%:1%:20%.

[0042] Battery assembly: Weigh 0.40 g of the magnetically induced lithium-rich manganese-based positive electrode material prepared in Example 1, add 0.05 g of conductive carbon black as a conductive agent and 0.05 g of polyvinylidene fluoride as a binder to prepare a positive electrode slurry; weigh 0.40 g of the graphene-coated lithium titanate material prepared in Example 1, add 0.05 g of conductive carbon black as a conductive agent and 0.05 g of polyvinylidene fluoride as a binder to prepare a negative electrode slurry; add the electrolyte prepared in Example 1 dropwise.

[0043] The prepared slurry is coated, then rolled, slit and die-cut. The compaction density of the positive electrode is 3.6 g / cm 3 The compaction density of the negative electrode roller is 1.65g / cm 3 The die-cut positive and negative electrode sheets are stacked, encapsulated with aluminum-plastic film, dried, injected with liquid, formed, encapsulated with aluminum-plastic film again, and divided into different capacities to prepare a soft-pack full battery.

[0044] The electrochemical performance test shows that the assembled soft-pack full battery has a voltage range of 2.0 to 4.8 V and a 1 C (250 mAh g -1) and cycled 30 times at a rate of 1.154Ah at -25°C.

[0045] Comparative Case 1

[0046] The preparation method of a magnetically induced low-temperature starting lithium-ion battery comprises the following steps:

[0047] (1) Preparation of magnetically induced lithium-rich manganese-based positive electrode materials: nickel acetate, cobalt acetate and manganese acetate were added to 100 ml of distilled water according to a molar ratio of 0.13:0.13:0.54, and mixed evenly for 30 minutes at 50°C, 500 rpm / min, and a magnetic stirrer with a magnetic stirring of 200w; lithium hydroxide was added according to the lithium source: (nickel source + cobalt source + manganese source) = 1.56:1, and mixed evenly for 30 minutes at 50°C, 500 rpm / min, and a magnetic stirrer with a magnetic stirring of 200w; then evaporated at 110°C to form a mixed slurry. In an air atmosphere, the slurry was placed in a muffle furnace for calcination at a temperature of 500°C for 5 hours and at 850°C for 11 hours.

[0048] (2) Preparation of graphene-coated lithium titanate composite material: 5g of titanium dioxide was added to 500ml of ethanol and dispersed at 25°C and 100rpm / min for 30min; then 1ml of a 5mg / mL single-layer graphene mixed solution was slowly added; finally, 1.9g of lithium carbonate was added and evaporated at 85°C and 100rpm / min to a slurry. Under an argon atmosphere, the temperature was 800°C and the calcination time was 15h to obtain a graphene-coated lithium titanate composite material.

[0049] (3) Preparation of low-temperature electrolyte: the solute is 1.2 mol / L lithium hexafluorophosphate; the solvent is ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a ratio of 2:3:5 (w / w / w); the solute accounts for 25% of the solvent by mass percentage; the mass ratio of electrolyte additives propylene carbonate: ethylene carbonate: ethyl acetate is 5%:1%:20%.

[0050] Battery assembly: Weigh 0.40g of the lithium-rich manganese-based positive electrode material prepared in Comparative Example 1, add 0.05g of conductive carbon black as a conductive agent and 0.05g of polyvinylidene fluoride as a binder to prepare a positive electrode slurry; weigh 0.40g of the graphene-coated lithium titanate composite material prepared in Comparative Example 1, add 0.05g of conductive carbon black as a conductive agent and 0.05g of polyvinylidene fluoride as a binder to prepare a negative electrode slurry; add the electrolyte prepared in Comparative Example 1 dropwise.

[0051] The prepared slurry is coated, then rolled, slit and die-cut. The compaction density of the positive electrode is 3.6 g / cm 3 The compaction density of the negative electrode roller is 1.65g / cm 3The die-cut positive and negative electrode sheets are stacked, encapsulated with aluminum-plastic film, dried, injected with liquid, formed, encapsulated with aluminum-plastic film again, and divided into different capacities to prepare a soft-pack full battery.

[0052] The electrochemical performance test shows that the assembled soft-pack full battery has a voltage range of 2.0 to 4.8 V and a 1 C (250 mAh g -1 ) and cycled 30 times at a rate of 1.024Ah at -25°C.

[0053] Comparative Case 2

[0054] The preparation method of a magnetically induced low-temperature starting lithium-ion battery comprises the following steps:

[0055] (1) Preparation of magnetically induced lithium-rich manganese-based positive electrode materials: nickel acetate, cobalt acetate and manganese acetate were added to 100 ml of distilled water according to a molar ratio of 0.13:0.13:0.54, and mixed evenly for 30 minutes at 50°C, 50 rpm / min, and a magnetic stirrer with a magnetic stirring of 200w; lithium hydroxide was added according to the lithium source: (nickel source + cobalt source + manganese source) = 1.6:1, and mixed evenly for 30 minutes at 50°C, 50 rpm / min, and a magnetic stirrer with a magnetic stirring of 200w; then evaporated at 110°C to form a mixed slurry. In an air atmosphere, the slurry was placed in a muffle furnace for calcination at a temperature of 500°C for 5 hours and at 900°C for 12 hours.

[0056] (2) Preparation of lithium titanate: 5 g of titanium dioxide was added to 500 ml of ethanol and dispersed at 25°C and 100 rpm / min for 180 min. Then 1.9 g of lithium carbonate was added and evaporated at 85°C and 100 rpm / min until it became a slurry. Finally, lithium titanate was obtained under an argon atmosphere at a temperature of 800°C and a calcination time of 10 h.

[0057] (3) Preparation of low-temperature electrolyte: the solute is 1.2 mol / L lithium hexafluorophosphate; the solvent is ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a ratio of 2:3:5 (w / w / w); the solute accounts for 25% of the solvent by mass percentage; the mass ratio of electrolyte additives propylene carbonate: ethylene carbonate: ethyl acetate is 5%:1%:20%.

[0058] Battery assembly: Weigh 0.40g of the magnetically induced lithium-rich manganese-based positive electrode material prepared in Comparative Example 2, add 0.05g of conductive carbon black as a conductive agent and 0.05g of polyvinylidene fluoride as a binder to prepare a positive electrode slurry; weigh 0.40g of the lithium titanate material prepared in Comparative Example 2, add 0.05g of conductive carbon black as a conductive agent and 0.05g of polyvinylidene fluoride as a binder to prepare a negative electrode slurry. Add the electrolyte prepared in Comparative Example 2 dropwise.

[0059] The prepared slurry is coated, then rolled, slit and die-cut. The compaction density of the positive electrode is 3.6 g / cm 3 The compaction density of the negative electrode roller is 1.65g / cm 3 The die-cut positive and negative electrode sheets are stacked, encapsulated with aluminum-plastic film, dried, injected with liquid, formed, encapsulated with aluminum-plastic film again, and divided into different capacities to prepare a soft-pack full battery.

[0060] The electrochemical performance test shows that the assembled soft-pack full battery has a voltage range of 2.0 to 4.8 V and a 1 C (250 mAh g -1 ) and cycled 30 times at a rate of 0.978 Ah at -25°C.

[0061] Comparative Case 3

[0062] The preparation method of a magnetically induced low-temperature starting lithium-ion battery comprises the following steps:

[0063] (1) Preparation of magnetically induced lithium-rich manganese-based positive electrode materials: nickel acetate, cobalt acetate and manganese acetate were added to 100 ml of distilled water according to a molar ratio of 0.13:0.13:0.54, and mixed evenly for 30 minutes at 50°C, 50 rpm / min, and a magnetic stirrer with a magnetic stirring of 200w; lithium hydroxide was added according to the lithium source: (nickel source + cobalt source + manganese source) = 1.55:1, and mixed evenly for 30 minutes at 50°C, 50 rpm / min, and a magnetic stirrer with a magnetic stirring of 200w; then evaporated at 110°C to form a mixed slurry. In an air atmosphere, the slurry was placed in a muffle furnace for calcination at a temperature of 500°C for 5 hours and at 900°C for 12 hours.

[0064] (2) Preparation of graphene-coated lithium titanate composite material: 5g of titanium dioxide was added to 500ml of ethanol and dispersed at 25°C and 100rpm / min for 30min; then 10ml of a 10mg / mL single-layer graphene mixed solution was slowly added; finally, 1.9g of lithium carbonate was added and evaporated at 85°C and 100rpm / min to a slurry. Under an argon atmosphere, the temperature was 1000°C and the calcination time was 8h to obtain a graphene-coated lithium titanate composite material.

[0065] (3) Preparation of electrolyte: the solute is 1.2 mol / L lithium hexafluorophosphate; the solvent is ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a ratio of 2:3:5 (w / w / w); the solute accounts for 25% of the solvent by mass percentage;

[0066] Battery assembly: Weigh 0.40g of the magnetically induced lithium-rich manganese-based positive electrode material prepared in Comparative Example 3, add 0.05g of conductive carbon black as a conductive agent and 0.05g of polyvinylidene fluoride as a binder to prepare the positive electrode slurry; weigh 0.40g of the graphene-coated lithium titanate composite material prepared in Comparative Example 3, add 0.05g of conductive carbon black as a conductive agent and 0.0500g of polyvinylidene fluoride as a binder to prepare the negative electrode slurry, and add the electrolyte prepared in Comparative Example 3 dropwise.

[0067] The prepared slurry is coated, then rolled, slit and die-cut. The compaction density of the positive electrode is 3.6 g / cm 3 The compaction density of the negative electrode roller is 1.65g / cm 3 The die-cut positive and negative electrode sheets are stacked, encapsulated with aluminum-plastic film, dried, injected with liquid, formed, encapsulated with aluminum-plastic film again, and divided into different capacities to prepare a soft-pack full battery.

[0068] The electrochemical performance test shows that the assembled soft-pack full battery has a voltage range of 2.0 to 4.8 V and a 1 C (250 mAh g -1 ) and cycled 30 times at a rate of 0.973 Ah at -25°C.

[0069] It can be clearly seen from the comparative experimental results and the drawings in the specification that, under low temperature conditions, the battery prepared by the method of the present invention has a larger discharge capacity than that of the battery and can remain stable when the number of cycles increases.

Claims

1. A low-temperature starting lithium-ion battery, characterized in that: Its composition includes magnetic induction positive electrode material, electrolyte and negative electrode material; The preparation method of the magnetic induction positive electrode material comprises the following steps: (1) dispersing the lithium source, nickel source, cobalt source and manganese source into a solvent, uniformly mixing them under a magnetic stirrer, evaporating them, and forming a mixed slurry under magnetic induction; The stirring conditions are as follows: stirring speed of 100-2000 rpm / min, stirring temperature of 20-100°C, and stirring time of 1-10 hours; the evaporation conditions are as follows: stirring speed of 100-2000 rpm / min, evaporation temperature of 80-180°C, and evaporation time of 8-24 hours; (2) calcining the mixed slurry twice and cooling it to form a lithium-rich manganese-based positive electrode material; The secondary calcination is carried out twice in an air atmosphere, the first calcination is carried out at a temperature of 350-500°C for 4-6 hours, and the second calcination is carried out at a temperature of 850-1000°C for 10-15 hours; The molar ratio of the nickel source, the cobalt source and the manganese source is 0.13:0.13:0.54; The ratio of the amount of lithium contained in the lithium source to the total amount of Ni, Co, and Mn in the lithium-rich manganese-based precursor is 1.5-1.6:1; The electrolyte is prepared by using ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate as the basic solution, and then adding additives; The additive accounts for 11-40% of the electrolyte by volume; the additive is added in a ratio of propylene carbonate: ethylene carbonate: ethyl acetate = 1-10%: 0.5-5%: 10-25% by volume; The method for preparing the negative electrode material comprises the following steps: (1) Add the titanium source to the buffer solution and disperse it by ultrasonication to form a mixed solution; (2) adding a single-sheet graphene dispersion to the mixed dispersion, adding a lithium source after continuous ultrasonic dispersion at room temperature, and centrifuging and washing to obtain a composite; (3) The composite is calcined at 600-1000°C in an inert atmosphere for 8-24 hours and then naturally cooled to obtain a graphene-coated lithium titanate composite material.

2. A low-temperature starting lithium-ion battery according to claim 1, characterized in that: The lithium source is at least one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium acetate dihydrate and lithium hydroxide monohydrate.

3. A low-temperature starting lithium-ion battery according to claim 1, characterized in that: The titanium source is one or both of titanium dioxide and tetrabutyl titanate; the buffer solution is one or more of ethanol, methanol or acetone.

4. A low-temperature starting lithium-ion battery according to claim 1, characterized in that: The concentration of the single-sheet graphene dispersion is 5-10 mg / mL, and the mass ratio of the composite to the single-sheet graphene is 10-100:1.