A three-dimensional lightweight lithium-philic current collector for lithium metal composite negative electrode and its preparation method and application

By using lightweight organic sponges or sponges as substrates in lithium metal batteries, metal nanoparticles are deposited to form dense nucleation site layers, which solves the dendrites and volume expansion problems of lithium metal batteries, and improves the energy density and cycle stability of the battery sex.

CN115881976BActive Publication Date: 2024-12-03CENT SOUTH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211426461.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-12-03
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

Lithium metal batteries are prone to dendrite, dead lithium and side reactions during charging and discharging, resulting in electrolyte consumption and rupture of solid electrolyte interface film, affecting battery performance. The existing three-dimensional current collectors are used to improve energy density and inhibit dendrite growth. There are problems of high mass density or poor lithium-philicity.

Method used

Using lightweight organic sponges or sponges as substrates, uniform metal nanoparticles are deposited by electroplating or electroplating to form dense nucleation site layers and conductive layers, promoting uniform dispersion and diffusion of lithium ions, reducing dendrites' growth and Volume expansion improves the cyclic stability of the electrode.

Benefits of technology

Effectively inhibit the growth of lithium dendrites, improve the energy density and effective capacity of the battery, enhance the uniform deposition and detachment of lithium metal, form a stable SEI film, and extend the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115881976B_ABST
    Figure CN115881976B_ABST
Patent Text Reader

Abstract

The present invention provides a three-dimensional light lithium-philic current collector for lithium metal composite negative electrode and its preparation method and application. The preparation method comprises the following steps: (1) making a block of organic sponge or sponge-like organic skeleton into a disc, and washing and drying it; (2) then depositing metal nanoparticles on the surface of the obtained disc, taking it out, washing and drying it, and obtaining the three-dimensional light lithium-philic current collector for lithium metal composite negative electrode. The present invention promotes the uniform deposition and stripping of lithium metal by designing a light three-dimensional current collector, and effectively solves the outstanding problems such as dendrite growth, reaction with electrolyte, and volume expansion during the charging and discharging process of lithium metal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and in particular relates to a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode, and a preparation method and application thereof. Background Art

[0002] With the development of society, people require higher mileage for power tools, which means higher energy density is needed for energy storage systems. However, the current energy storage system lithium-ion batteries cannot meet the needs of new power equipment due to their limited energy density. Lithium metal has a higher specific capacity (3860mA hg -1 ), a low electrode potential (-3.04 V vs standard hydrogen electrode) and the smallest density among metals (0.534 g cm -3 ) is an ideal negative electrode material for energy storage batteries. However, due to the fact that lithium metal batteries are prone to produce dendrites and dead lithium during the charging and discharging process, and the extremely high reactivity of lithium metal itself, it is very easy to react with the electrolyte during the charging and discharging process to generate an unstable solid electrolyte interface film, causing the consumption of electrolyte. At the same time, since it is a host-free negative electrode, it is very easy to cause volume expansion during the charging and discharging process, causing the generated solid electrolyte interface film to rupture and regenerate, thereby forming a thick SEI film on the interface, causing a decrease in battery performance, which hinders the practical application of lithium metal batteries.

[0003] In response to the problems of lithium metal batteries such as dendrite growth, reaction with electrolyte and volume expansion, the current solution strategy is mainly to promote the uniform deposition of lithium metal and inhibit the growth of lithium dendrites through electrolyte modification (adding additives with different functions), constructing artificial SEI membranes and three-dimensional current collectors. In particular, three-dimensional current collectors can effectively disperse local current density, increase the specific surface area of ​​the electrode, promote the uniform deposition of lithium metal, and inhibit the growth of lithium dendrites. Therefore, they are favored by many researchers.

[0004] The three-dimensional current collectors (skeletons) currently used are mainly divided into two categories: metal-based and carbon-based. Although the metal-based (copper, copper-zinc alloy, stainless steel, etc.) has good mechanical properties, it has a large mass density and accounts for a large proportion in the electrode, which greatly reduces the energy density of the battery. For example, Jinkui Feng and other researchers from Shandong University used a one-step vacuum distillation method to prepare a three-dimensional porous copper current collector. By regulating the size of the pores of the porous structure, the growth of dendrites and the volume expansion of lithium metal were effectively suppressed; carbon-based (carbon fiber, carbon cloth, carbon paper, etc.) have certain flexibility and low mass density, which can effectively improve the energy density of the battery, but their lithium affinity is poor, which seriously affects the lithium deintercalation and electrochemical properties. The lithium-philic functional group can promote the uniform deposition of lithium and effectively inhibit the growth of dendrites. Zhang Qiang and other researchers from Tsinghua University introduced lithium-philic functional groups through nitrogen-doped graphene to induce uniform nucleation and deposition of lithium, thereby inhibiting the growth of lithium dendrites; Huang from Huazhong University of Science and Technology Yunhui and other researchers loaded silver nanowires onto a melamine sponge skeleton through a self-assembly method. The silver nanowires acted as nucleation units to regulate the deposition of lithium, thereby inhibiting the growth of lithium dendrites. However, silver nanowires have the disadvantages of uneven distribution and loose nucleation sites in the three-dimensional structure, which is not conducive to the performance of the battery. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology, and provide a three-dimensional lightweight lithium-philic current collector for lithium metal composite negative electrode and its preparation method and application. The present invention promotes the uniform deposition and stripping of lithium metal by designing a lightweight three-dimensional current collector, thereby effectively solving the prominent problems such as dendrite growth, reaction with electrolyte, and volume expansion during the charging and discharging process of lithium metal batteries.

[0006] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0007] A method for preparing a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode comprises the following steps:

[0008] (1) forming a block of organic sponge or sponge-like organic skeleton into a disc, and washing and drying the disc;

[0009] (2) Then, metal nanoparticles are deposited on the surface of the obtained disc, which is taken out, cleaned, and dried to obtain the three-dimensional lightweight lithium-philic current collector for the lithium metal composite negative electrode.

[0010] The present invention uses cheap organic sponge or sponge-like organic structure as a matrix, and deposits uniform metal nanoparticles on its surface by electroless plating, electroplating, magnetron sputtering, etc., especially the unique and uniform particle morphology characteristics of the sponge surface (such as Figure 1 ), leading to the formation of a dense nucleation site layer and a conductive layer (as shown in Figure 2As shown), thus forming a lightweight organic three-dimensional lithium-philic conductive current collector. The unique capillary action of the sponge is used to absorb the electrolyte into the pores of the three-dimensional current collector, so that the lithium ions are evenly dispersed in the electrode structure, which plays a role in evenly dispersing lithium ions, thereby accelerating the diffusion rate of lithium ions in the electrode during the charge and discharge process, reducing the concentration difference of lithium ions during the charge and discharge process, promoting the uniform deposition and release of lithium metal, forming a stable SEI film, effectively reducing the side reaction between lithium metal and the electrolyte, and stabilizing the cycle stability of the electrode. At the same time, due to the formation of a dense and uniform nucleation site layer, the nucleation overpotential can be effectively reduced. At the same time, a large number of nucleation sites provide effective spatial sites for the deposition of lithium, promoting the uniform deposition of lithium metal in the three-dimensional current collector. The fast lithium ion diffusion channel formed provides effective conditions for the stripping of lithium ions, laying a solid foundation for the long-term cycle of the battery.

[0011] The three-dimensional lightweight lithium-philic current collector of the present invention effectively reduces the local current density, increases the specific surface area of ​​the negative electrode, and can effectively inhibit the growth of lithium dendrites. The sponge flexibility can release the stress generated during the lithium deposition process, thereby further inhibiting the growth of dendrites. At the same time, the three-dimensional skeleton structure can effectively alleviate the volume expansion problem of lithium metal during the charge and discharge process. In addition, the uniformly deposited metal nanoparticles provide a large number of nucleation sites, reduce the nucleation overpotential of lithium, and provide necessary conditions for the uniform deposition of lithium.

[0012] Preferably, in step (1), the organic sponge is a melamine sponge; and the sponge-like organic skeleton is a sponge-like PVA synthetic absorbent towel.

[0013] Preferably, the density of the melamine sponge is 20-22 mg / cm 3 , total hole area is 2-2.5m 2 / g, the porosity is 98-99%; the density of the sponge-like PVA synthetic absorbent towel is 21-23mg / cm 3 Further preferably, the density of the melamine sponge is 20.69 mg / cm 3 , the total hole area is 2.226m 2 / g, the porosity is 98.41%; the density of the sponge-like PVA synthetic absorbent towel is 22.5mg / cm 3 .

[0014] Preferably, in step (2), the metal nanoparticles include metal single substance nanoparticles composed of one of gold, silver, magnesium, copper, zinc, aluminum, tin, platinum, nickel, and silicon, or metal alloy nanoparticles composed of at least two of them.

[0015] Preferably, the metal nanoparticles are silver nanoparticles; depositing the metal nanoparticles on the surface of the obtained disc specifically comprises the following steps: soaking the disc in a silver ammonia solution with a concentration of 0.05-0.25 mol / L for 20-60 minutes, and then placing it in a glucose solution with a concentration of 0.015-0.085 mol / L for reaction for 2-10 minutes. The above-mentioned process of depositing metal nanoparticles on the surface is combined with the melamine sponge with specific properties of the present invention, and a dense metal nanoparticle layer of a certain size can be more evenly deposited on the surface of the sponge, and the obtained product has better performance.

[0016] Preferably, the metal nanoparticles are metal single substance nanoparticles composed of one of gold, tin and nickel; depositing the metal nanoparticles on the surface of the obtained wafer specifically comprises the following steps: plating dense gold nanoparticles on the surface of the wafer by magnetron sputtering, the background vacuum degree of the magnetron sputtering method is 4*10 -4 -6*10 -4 Pa, the sputtering current is 0.6-2.0A, the coating temperature is 25-180℃, the coating time is 30-120s, and the sputtering gas pressure is 0.4-1.0Pa.

[0017] Preferably, in step (1), the diameter of the disc is 12-16 mm and the thickness is 1-3 mm.

[0018] Preferably, in step (1), the cleaning is ultrasonic cleaning with deionized water, and the number of cleaning times is 3-5 times; the drying is vacuum drying, and the drying temperature is 60-100°C; in step (2), the cleaning is cleaning with deionized water, and the number of cleaning times is 3-5 times; the drying is vacuum drying, and the drying temperature is 60-100°C.

[0019] As a general inventive concept, the present invention provides a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode prepared by the above-mentioned preparation method.

[0020] As a general inventive concept, the present invention provides an application of the above-mentioned three-dimensional lightweight lithium-philic current collector for lithium metal composite negative electrode, and uses the three-dimensional lightweight lithium-philic current collector for lithium metal composite negative electrode to prepare lithium metal button battery, including the following steps: assembling a button battery in the order of a positive electrode shell, a three-dimensional lightweight lithium-philic current collector for lithium metal composite negative electrode, a separator, a lithium sheet, and a negative electrode shell, and dripping an electrolyte during the assembly process.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention utilizes the unique structural structure of a lightweight self-supporting organic sponge or a sponge-like organic skeleton to uniformly deposit a dense metal nanoparticle layer (nucleation site layer) of a certain size on its surface, providing a large number of nucleation sites and spatial structures for the deposition of lithium, effectively inhibiting the growth and volume change of lithium dendrites, and effectively improving the energy density and effective capacity of the battery. It is an innovative method and effective strategy to solve the problems that limit the practical application of lithium metal batteries and improve the energy density of batteries.

[0023] (2) The present invention constructs a lightweight, lithium-philic composite host skeleton from an organic sponge or sponge-like organic skeleton with a certain flexibility through surface modification, which not only avoids the shortcomings of low energy density of metal-based current collector batteries and poor lithium affinity of carbon-based current collectors, but also gives the lithium-philic skeleton a new characteristic of flexibility, broadening the application field of batteries. At the same time, its elastic structural characteristics will effectively and evenly disperse the electrolyte (lithium ions) inside the battery, providing a good environment for further promoting the uniform deposition of lithium ions, achieving uniform deposition of lithium and long-term circulation of the negative electrode, and providing a reference for the design of composite lithium metal negative electrodes. This is an innovation in the research method of lithium negative electrodes. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is a surface morphology of the melamine sponge in Example 1;

[0026] Figure 2 This is a surface morphology of the three-dimensional lightweight lithium-philic current collector in Example 1;

[0027] Figure 3 Surface image (left) and cross-sectional image (right) of uniform deposition of lithium metal in the three-dimensional lightweight lithium-philic current collector of Example 1;

[0028] Figure 4 This is a surface morphology of the three-dimensional lightweight lithium-philic current collector in Example 3;

[0029] Figure 5 This is a comparison chart of the coulombic efficiency test of the button cell in Example 1 and Comparative Example 1;

[0030] Figure 6 It is a comparison diagram of symmetrical battery tests of button batteries in Example 1 and Comparative Example 1;

[0031] Figure 7This is a comparison chart of the full battery test corresponding to Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0032] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0033] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0035] Embodiment 1:

[0036] A method for preparing a three-dimensional lightweight lithium-philic current collector (experimental group) for a lithium metal composite negative electrode comprises the following steps:

[0037] (1) The block melamine sponge was cut into discs with a diameter of 14 mm and a thickness of 2 mm, and ultrasonically cleaned three times with deionized water and then vacuum dried at 60°C; the density of the block melamine sponge was 20.69 mg / cm 3 , total hole area 2.226m 2 / g, porosity is 98.41%;

[0038] (2) using a silver mirror reaction method to deposit dense silver nanoparticles on the surface of the wafer by an electroless plating method, specifically comprising the following steps: first, soaking the dried wafer in a 0.15 mol / L silver ammonia solution for 60 min, and then placing it in a 0.1 mol / L glucose solution for reaction for 10 min;

[0039] (3) The wafer after the reaction was taken out, washed with deionized water for three times, and dried at 60° C. in a vacuum oven for 12 hours for later use, thereby preparing a three-dimensional lightweight lithium-philic current collector (skeleton).

[0040] The surface morphology of the above melamine sponge is shown in FIG. Figure 1 As shown; the surface morphology of the prepared three-dimensional lightweight lithium-philic current collector is shown Figure 2 shown.

[0041] Preparation of lithium metal batteries:

[0042] The prepared three-dimensional lightweight lithium-philic current collector (skeleton), separator, lithium sheet, and battery shell are assembled into a button battery in the order of positive electrode shell, three-dimensional lightweight lithium-philic current collector, separator, lithium sheet, and negative electrode shell. Two drops of electrolyte are added during the assembly process. The assembled button battery is left to stand for 12 hours before the electrochemical performance test.

[0043] Surface image (left) and cross-sectional image (right) of uniform deposition of lithium metal in a three-dimensional lightweight lithium-philic current collector (1 mAh cm -2 )like Figure 3 shown.

[0044] Comparative Example 1:

[0045] Battery preparation:

[0046] (1) Commercial copper foam was cut into discs with a diameter of 14 mm and a thickness of 2 mm, ultrasonically cleaned three times with deionized water, and then vacuum dried at 60°C;

[0047] (2) The copper foam, separator, lithium sheet, and battery shell are assembled into a button cell (i.e., half-cell) in the order of positive electrode shell, three-dimensional current collector, separator, lithium sheet, and negative electrode shell. Two drops of electrolyte are added during the assembly process. The assembled button cell is left to stand for 12 hours before the electrochemical performance test is performed.

[0048] The button cell in Example 1 and the button cell in Comparative Example 1 were subjected to electrochemical performance tests, including coulomb efficiency test, symmetric cell test, and full cell test.

[0049] (1) Coulomb efficiency test

[0050] After standing for 12 hours, the button cell was charged at 1 mA cm -2 The current density is 1 mAh cm -2 The coulombic efficiency test was carried out at a capacity of Figure 5 The coulomb efficiency test comparison diagram of the button cell in Example 1 (corresponding to the Ag@PMS in the figure) and Comparative Example 1 (corresponding to the Cu foam in the figure) is shown in FIG. Figure 5 It can be seen that the technical solution of Example 1 has better lithium insertion and extraction ability and cycle stability than that of Comparative Example 1, and still maintains a coulombic efficiency of 97.14% after 450 cycles.

[0051] (2) Symmetrical battery test

[0052] After standing for 12 hours, the button cell was first charged with a small current of 0.5 mA cm -2 Current density of 10 mA h cm deposited in three-dimensional lightweight lithium-philic current collector (skeleton) and copper foam -2 capacity, then at 1 mA cm -2The current density is 1 mAh cm -2 The voltage stability of the composite lithium metal negative electrode of the present invention is demonstrated by a cycle test at a capacity of Figure 6 The symmetrical battery test comparison diagram of the button battery in Example 1 (corresponding to the Ag@PMS in the figure) and Comparative Example 1 (corresponding to the Cu foam in the figure) is shown in FIG. Figure 6 It can be seen that after Example 1 has been cycled for 3300 hours, the voltage still maintains excellent stability, and the average polarization voltage is only 31.5mV. However, in Comparative Example 1, not only the polarization voltage is large, but also the battery short-circuited after 230 cycles, indicating that the negative electrode is extremely unstable, which is not conducive to the deposition and release of lithium. A large number of dendrites are generated during the cycle, resulting in short circuit and failure of the battery.

[0053] (3) Full battery test

[0054] After the button cell (i.e., half-cell) was assembled and left to stand for 12 h, 5 mA h cm was pre-deposited in the three-dimensional lightweight lithium-philic current collector (skeleton) and copper foam. -2 The lithium metal is used to obtain a composite lithium metal negative electrode, which is then disassembled and assembled with a lithium iron phosphate positive electrode into a full battery. The cycle test is carried out at a current density of 3C. Figure 7 As shown, the experimental group corresponding to Example 1 (corresponding to the Ag@PMS in the figure) has good cycle stability, and still has a capacity retention rate of 76.5% after 300 cycles, while the capacity of the comparison group corresponding to Comparative Example 1 (corresponding to the Cu foam in the figure) begins to decay rapidly after 100 cycles, and the capacity retention rate is only 73.7% after 200 cycles, indicating that the scheme of the present invention has good practical application effect and value.

[0055] Embodiment 2:

[0056] A method for preparing a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode comprises the following steps:

[0057] (1) The block melamine sponge was cut into discs with a diameter of 12 mm and a thickness of 2 mm, and ultrasonically cleaned three times with deionized water and then vacuum dried at 60°C; the density of the block melamine sponge was 20.69 mg / cm 3 , total hole area 2.226m 2 / g, porosity is 98.41%;

[0058] (2) using a silver mirror reaction method to deposit dense silver nanoparticles on the surface of the wafer by an electroless plating method, specifically comprising the following steps: firstly, soaking the dried wafer in a 0.05 mol / L silver ammonia solution for 20 min, and then placing it in a 0.025 mol / L glucose solution for reaction for 2 min;

[0059] (3) The wafer after the reaction was taken out, washed with deionized water for three times, and dried at 60° C. in a vacuum oven for 12 hours for later use, thereby preparing a three-dimensional lightweight lithium-philic current collector (skeleton).

[0060] Preparation of lithium metal batteries:

[0061] The prepared three-dimensional lightweight lithium-philic current collector (skeleton), separator, lithium sheet, and battery shell are assembled into a button battery in the order of positive electrode shell, three-dimensional lightweight lithium-philic current collector, separator, lithium sheet, and negative electrode shell. Two drops of electrolyte are added during the assembly process. The assembled button battery is left to stand for 12 hours before the electrochemical performance test.

[0062] Embodiment 3:

[0063] A method for preparing a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode comprises the following steps:

[0064] (1) The block melamine sponge was cut into discs with a diameter of 14 mm and a thickness of 2 mm, and ultrasonically cleaned three times with deionized water and then vacuum dried at 60°C; the density of the block melamine sponge was 20.69 mg / cm 3 , total hole area 2.226m 2 / g, porosity is 98.41%;

[0065] (2) using a silver mirror reaction method to deposit dense silver nanoparticles on the surface of the wafer by an electroless plating method, specifically comprising the following steps: firstly, soaking the dried wafer in a 0.25 mol / L silver ammonia solution for 40 min, and then placing it in a 0.085 mol / L glucose solution for reaction for 5 min;

[0066] (3) Take out the wafer after the reaction, wash it with deionized water for 3 times, and dry it at 60°C in vacuum for 12 hours for standby use, thus preparing a three-dimensional light lithium-philic current collector (skeleton). Figure 4 shown.

[0067] Preparation of lithium metal batteries:

[0068] The prepared three-dimensional lightweight lithium-philic current collector (skeleton), separator, lithium sheet, and battery shell are assembled into a button battery in the order of positive electrode shell, three-dimensional lightweight lithium-philic current collector, separator, lithium sheet, and negative electrode shell. Two drops of electrolyte are added during the assembly process. The assembled button battery is left to stand for 12 hours before the electrochemical performance test.

[0069] Embodiment 4:

[0070] A method for preparing a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode comprises the following steps:

[0071] (1) The block melamine sponge was cut into discs with a diameter of 14 mm and a thickness of 2 mm, and ultrasonically cleaned three times with deionized water and then vacuum dried at 60°C; the density of the block melamine sponge was 20.69 mg / cm 3 , total hole area 2.226m 2 / g, porosity is 98.41%;

[0072] (2) The magnetron sputtering method is used to plate dense gold nanoparticles on the surface of the wafer. The background vacuum degree of the magnetron sputtering method is 4*10 -4 Pa, the sputtering current is 1.2A, the coating temperature is 25°C, the coating time is 30s, and the sputtering pressure is 0.4Pa, so that a three-dimensional lightweight lithium-philic current collector (skeleton) is prepared.

[0073] Preparation of lithium metal batteries:

[0074] The prepared three-dimensional lightweight lithium-philic current collector (skeleton), separator, lithium sheet, and battery shell are assembled into a button battery in the order of positive electrode shell, three-dimensional lightweight lithium-philic current collector, separator, lithium sheet, and negative electrode shell. Two drops of electrolyte are added during the assembly process. The assembled button battery is left to stand for 12 hours before the electrochemical performance test.

[0075] Embodiment 5:

[0076] A method for preparing a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode comprises the following steps:

[0077] (1) The block-like sponge-like PVA synthetic absorbent towel was cut into a disc with a diameter of 14 mm and a thickness of 2 mm, and ultrasonically cleaned with deionized water for 3 times and then vacuum dried at 60°C; the block-like sponge-like PVA synthetic absorbent towel had a 22.5 mg / cm 3 ;

[0078] (2) The magnetron sputtering method is used to plate dense tin nanoparticles on the surface of the wafer. The background vacuum degree of the magnetron sputtering method is 5*10 -4 Pa, the sputtering current is 0.6A, the coating temperature is 60°C, the coating time is 60s, and the sputtering pressure is 0.8Pa, so that a three-dimensional lightweight lithium-philic current collector (skeleton) is prepared.

[0079] Preparation of lithium metal batteries:

[0080] The prepared three-dimensional lightweight lithium-philic current collector (skeleton), separator, lithium sheet, and battery shell are assembled into a button battery in the order of positive electrode shell, three-dimensional lightweight lithium-philic current collector, separator, lithium sheet, and negative electrode shell. Two drops of electrolyte are added during the assembly process. The assembled button battery is left to stand for 12 hours before the electrochemical performance test.

[0081] Embodiment 6:

[0082] A method for preparing a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode comprises the following steps:

[0083] (1) The block-like three-type sponge PVA synthetic absorbent towel was cut into discs with a diameter of 14 mm and a thickness of 2 mm, ultrasonically cleaned with deionized water for 3 times, and then vacuum dried at 60°C; the block-like sponge PVA synthetic absorbent towel had a 22.5 mg / cm 3 ;

[0084] (2) The magnetron sputtering method is used to plate dense nickel nanoparticles on its surface. The background vacuum degree of the magnetron sputtering method is 6*10 -4 Pa, the sputtering current is 2A, the coating temperature is 180°C, the coating time is 120s, and the sputtering pressure is 1.0Pa, so that a three-dimensional lightweight lithium-philic current collector (skeleton) is prepared.

[0085] Preparation of lithium metal batteries:

[0086] The prepared three-dimensional lightweight lithium-philic current collector (skeleton), separator, lithium sheet, and battery shell are assembled into a button battery in the order of positive electrode shell, three-dimensional lightweight lithium-philic current collector, separator, lithium sheet, and negative electrode shell. Two drops of electrolyte are added during the assembly process. The assembled button battery is left to stand for 12 hours before the electrochemical performance test.

Claims

1. A method for preparing a three-dimensional lightweight lithium-philic current collector for a lithium metal composite negative electrode, characterized in that: The following steps are involved: (1) Forming a block of organic sponge or sponge-like organic skeleton into a disc, and then washing and drying it; (2) then depositing metal nanoparticles on the surface of the obtained disc, taking it out, cleaning it, and drying it to obtain the three-dimensional lightweight lithium-philic current collector for the lithium metal composite negative electrode; The metal nanoparticles are metal single substance nanoparticles composed of one of gold, tin and nickel. Depositing the metal nanoparticles on the surface of the obtained wafer specifically comprises the following steps: plating dense gold nanoparticles on the surface of the wafer by magnetron sputtering, and the background vacuum degree of the magnetron sputtering method is 4×10 -4 -6×10 -4 Pa, sputtering current is 0.6-2.0A, coating temperature is 25-180℃, coating time is 30-120s, sputtering pressure is 0.4-1.0Pa; In step (1), the cleaning is performed by ultrasonic cleaning with deionized water for 3-5 times; the drying is performed by vacuum drying at a temperature of 60-100°C; in step (2), the cleaning is performed by deionized water for 3-5 times; the drying is performed by vacuum drying at a temperature of 60-100°C.

2. The preparation method according to claim 1, characterized in that: In step (1), the organic sponge is a melamine sponge; and the sponge-like organic skeleton is a sponge-like PVA synthetic absorbent towel.

3. The preparation method according to claim 2, characterized in that: The density of the melamine sponge is 20-22 mg / cm 3 , total hole area is 2-2.5m 2 / g, the porosity is 98-99%; the density of the sponge-like PVA synthetic absorbent towel is 21-23mg / cm 3 .

4. The preparation method according to claim 1, characterized in that: The metal nanoparticles are silver nanoparticles; depositing the metal nanoparticles on the surface of the obtained disc specifically includes the following steps: soaking the disc in a silver ammonia solution with a concentration of 0.05-0.25 mol / L for 20-60 minutes, and then placing it in a glucose solution with a concentration of 0.015-0.085 mol / L for reaction for 2-10 minutes.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step (1), the diameter of the disc is 12-16 mm and the thickness is 1-3 mm.

6. A three-dimensional lightweight lithium-philic current collector for lithium metal composite negative electrode prepared by the preparation method as claimed in any one of claims 1 to 5.

7. An application of the three-dimensional lightweight lithium-philic current collector for lithium metal composite negative electrode as claimed in claim 6, characterized in that: The lithium metal button battery is prepared by using the three-dimensional lightweight lithium-philic current collector for the lithium metal composite negative electrode, comprising the following steps: assembling a button battery in the order of a positive electrode shell, a three-dimensional lightweight lithium-philic current collector for the lithium metal composite negative electrode, a separator, a lithium sheet, and a negative electrode shell, and dripping an electrolyte during the assembly process.

Citation Information

Patent Citations

  • Negative active material for lithium-ion secondary cell and preparation method thereof, and lithium-ion secondary cell

    CN107845781A

  • Rambutan shell-like 3D lithium-philic composite current collector, lithium metal anode and preparation and application thereof

    CN111816881A

  • Lithium metal-based battery taking copper selenide in-situ coated foamy copper as lithium metal carrier and preparation method of lithium metal-based battery

    CN112421115A

  • Lithium metal secondary battery, and negative terminal and porous copper current collector thereof

    WO2017181532A1