Curable resin composition, fuel cell, and sealing method

Solid polymer fuel cell sealant is solved by using a curable resin composition containing (meth)acryloyl and -[CH2C(CH3)2]-units in screen printing, and a curable resin composition of silicone compounds. The problems of repulsion and poor bubble defoaming in screen printing have achieved efficient sealing layer formation and are suitable for sealing purposes such as fuel cells.

CN115885122BActive Publication Date: 2024-11-12THREE BOND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180050950.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-31
Filing Date
2021-07-14
Publication Date
2024-11-12
Estimated Expiration
2041-07-14

AI Technical Summary

Technical Problem

The existing solid polymer fuel cell sealants have repulsion phenomena and poor bubble defoaming during screen printing, resulting in low coating efficiency and difficult to meet the requirements of production beat time.

Method used

A curable resin composition using a polyisobutyl resin containing (meth)acryloyl and -[CH2C(CH3)2]-unit, a free radical polymerization initiator, and a silicone compound defoaming agent without organic solvents, is passed through the wire Screen printing coats and cures with active energy rays to form a high-strength, high-extension sealing layer.

Benefits of technology

It realizes a curable resin composition suitable for screen printing while maintaining high strength and high extension characteristics, and improves the sealing property and coating efficiency of the sealing layer, and is suitable for sealing purposes such as fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115885122B_ABST
    Figure CN115885122B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a curable resin composition that can cope with coating based on screen printing while maintaining high strength and high elongation properties of the cured product. The curable resin composition contains the following (A) to (C) components. (A) component: containing one or more (meth)acryloyl groups and -[CH 2 C(CH 3 ) 2 ]-unit polyisobutylene resin; (B) component: a free radical polymerization initiator; (C) component: a defoaming agent containing a silicone compound that does not have a methoxysilyl group, an ethoxysilyl group and a (meth)acryloyl group and does not contain an organic solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a curable resin composition, a fuel cell and a sealing method. Background Art

[0002] In recent years, fuel cells have attracted attention as a new energy system for automobiles and homes. A fuel cell is a power generation device that extracts electrical energy by chemically reacting hydrogen and oxygen. In addition, as far as fuel cells are concerned, they are a clean next-generation power generation device because they have high energy efficiency when generating electricity and produce water through the reaction of hydrogen and oxygen. There are four types of fuel cells: solid polymer fuel cells, phosphoric acid fuel cells, molten carbonate fuel cells, and solid oxide fuel cells. Among them, solid polymer fuel cells are expected to be used in automotive power sources, household power generation devices, small power sources for electronic devices such as mobile phones, emergency power sources, etc. because their operating temperature is relatively low (around 80°C) and their power generation efficiency is high.

[0003] like Figure 1 As shown, the battery cell 1 of the solid polymer fuel cell has a structure including an electrolyte membrane electrode assembly (MEA) 5, a frame 6 supporting the MEA, and a diaphragm 2 forming a gas flow path, wherein the electrolyte membrane electrode assembly (MEA) 5 has a structure in which a polymer electrolyte membrane 4 is sandwiched between an air electrode (cathode) 3a and a fuel electrode (anode) 3b.

[0004] In order to start a solid polymer fuel cell, it is necessary to supply a fuel gas containing hydrogen to the anode and an oxidizing gas containing oxygen to the cathode in a separately isolated form. This is because there is a risk that if the isolation is insufficient, the gas on one side will mix with the gas on the other side, resulting in a decrease in power generation efficiency. Based on this background, sealants are mostly used to prevent leakage of fuel gas, oxidizing gas, etc. Specifically, sealants are used between adjacent diaphragms, between diaphragms and frames, between frames and electrolyte membranes or MEA, etc.

[0005] As a sealant used in a solid polymer fuel cell, a polymer composition using a polyisobutylene polymer is used because it is a rubber elastic body with excellent gas permeability resistance, low moisture permeability, heat resistance, and acid resistance. Specifically, Patent Document 1 discloses a polymer composition containing a telechelic polyisobutylene polymer having a terminal acrylate group and a reactive diluent, and having excellent cured product properties of high strength and high elongation.

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 2-88614 Summary of the invention

[0008] In recent years, in the manufacturing site, the coating of sealant, the curing process require the production tact time (tact time) to be further shortened. Specifically, from the viewpoint of productivity, screen printing (refer to Japanese Patent Publication No. 2009-117314) will be supported. However, the polymer composition of patent document 1 uses a high molecular weight polymer to improve the cured product characteristics such as high strength and high extension, so when the coating based on screen printing can be repelled from the adherend (repellence), or it is difficult to defoam the bubbles occurring in screen printing, which is not suitable for screen printing.

[0009] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a curable resin composition that can be applied by screen printing while maintaining high strength and high elongation properties of a cured product.

[0010] The gist of the present invention is described below.

[0011] [1] A curable resin composition comprising the following components (A) to (C):

[0012] Component (A): a polyisobutylene resin containing one or more (meth)acryloyl groups and -[CH2C(CH3)2]- units

[0013] Component (B): Radical polymerization initiator

[0014] (C) Component: A defoaming agent containing a silicone compound having no methoxysilyl group, no ethoxysilyl group, and no (meth)acryloyl group and containing no organic solvent.

[0015] [2] The curable resin composition according to [1], wherein the component (A) is a polyisobutylene resin represented by the general formula (1),

[0016] [Chemistry 1]

[0017]

[0018] (In formula (1), R 1 represents a monovalent or polyvalent aromatic hydrocarbon group, or a monovalent or polyvalent aliphatic hydrocarbon group which may have an aromatic ring, PIB represents a polyisobutylene skeleton containing the above-mentioned -[CH2C(CH3)2]- unit, R 4 represents a divalent hydrocarbon group having 2 to 6 carbon atoms which may contain an oxygen atom, R 2 and R 3 Each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms, and R 5 represents a hydrogen atom, a methyl group or an ethyl group, and n is an arbitrary integer from 1 to 6. ).

[0019] [3] The curable resin composition according to [1] or [2], comprising 0.1 to 10 parts by mass of the component (C) based on 100 parts by mass of the component (A).

[0020] [4] The curable resin composition according to any one of [1] to [3], further comprising a monofunctional monomer as the component (D).

[0021] [5] The curable resin composition according to any one of [1] to [4], which does not contain an organic solvent.

[0022] [6] In the curable resin composition according to any one of [1] to [5], the silicone compound of the component (C) is a compound having any structure of dimethylsiloxane, methylphenylsiloxane or diphenylsiloxane.

[0023] [7] The curable resin composition according to any one of [4] to [6], comprising 0.1 to 9 parts by mass of the component (C) based on 100 parts by mass of the total amount of the components (A) and (D).

[0024] [8] In the curable resin composition according to any one of [1] to [7], the component (B) is a photoradical polymerization initiator or an organic peroxide.

[0025] [9] A curable sealant for a fuel cell comprising the curable resin composition according to any one of [1] to [8].

[0026]

[10] The curable sealant for a fuel cell described in [9] is used for any component selected from the group consisting of a diaphragm, a frame, an electrolyte membrane, a fuel electrode, an air electrode, and an electrolyte membrane electrode assembly as components in a fuel cell.

[0027]

[11] A cured product of the curable resin composition according to any one of [1] to [8].

[0028]

[12] A fuel cell comprising any seal selected from the group consisting of a seal between adjacent diaphragms in the fuel cell and a seal between a frame of the fuel cell and an electrolyte membrane or an electrolyte membrane electrode assembly, wherein the above-mentioned any seal is a solidified material described in

[11] .

[0029]

[13] A sealing method for sealing at least a portion between at least two flanges of a sealed component having at least two flanges, wherein at least one of the flanges is permeable to active energy rays, the sealing method comprising: a step of coating a curable resin composition as described in any one of [1] to [8] on a surface of at least one of the flanges, a step of bonding one flange coated with the curable resin composition and another flange via the curable resin composition, and a step of irradiating the flange permeable to active energy rays with active energy rays to cure the curable resin composition, thereby sealing at least a portion between the at least two flanges.

[0030]

[14] A sealing method for sealing at least a portion between at least two flanges of a sealed component having at least two flanges, the sealing method comprising: a step of applying the curable resin composition described in any one of [1] to [8] to at least one of the flanges, a step of irradiating the applied curable resin composition with active energy rays to cure the curable resin composition, thereby forming a gasket containing a cured product of the curable resin composition, and a step of placing another flange on the gasket and crimping the one flange coated with the curable resin composition and the other flange with the gasket interposed therebetween, thereby sealing at least a portion between the at least two flanges.

[0031]

[15] A sealing method for sealing at least a portion between at least two flanges of a sealed component having at least two flanges, the sealing method comprising: a step of arranging a gasket forming mold on at least one of the flanges, a step of injecting a curable resin composition described in any one of [1] to [8] into at least a portion of a gap between the gasket forming mold and the one flange on which the mold is arranged, a step of irradiating the curable resin composition with the active energy rays to cure the curable resin composition, thereby forming a gasket containing a cured product of the curable resin composition, a step of removing the mold from the one flange, and a step of arranging another flange on the gasket and crimping the one flange and the other flange with the gasket clamped therebetween, thereby sealing at least a portion between the at least two flanges.

[0032] Effects of the Invention

[0033] The present invention provides a curable resin composition capable of being applied by screen printing while maintaining high strength and high elongation properties of a cured product. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a schematic cross-sectional view of a single cell unit of a fuel cell.

[0035] Figure 2 It is a schematic diagram showing the entire fuel cell. DETAILED DESCRIPTION

[0036] The present invention is described in detail below. It should be noted that, in this specification, the use of "X to Y" means that the numerical values ​​(X and Y) recorded before and after it are included as the lower limit and upper limit, and means "more than X and less than Y". In addition, the (meth)acrylate in the present invention refers to both acrylate and methacrylate.

[0037] The curable resin composition of the present invention contains: (A) component: a polyisobutylene resin containing one or more (meth)acryloyl groups and -[CH2C(CH3)2]- units, (B) component: a free radical polymerization initiator, and (C) component: a defoamer containing a silicone compound without a methoxysilyl group, an ethoxysilyl group, and a (meth)acryloyl group and containing no organic solvent. According to the present invention, a curable resin composition having high strength, high elongation and suitable for screen printing is provided. Suitable for screen printing means, for example, having the property that it will not be repelled from the adherend during the application of screen printing and that bubbles will not be generated due to screen printing.

[0038] <(A)Component>

[0039] The component (A) used in the present invention is not particularly limited as long as it is a polymer having a polyisobutylene skeleton containing one or more (meth)acryloyl groups and -[CH2C(CH3)2]- units. The component (A) may have, for example, a -[CH2C(CH3)2]- unit (polyisobutylene skeleton), and may be a polymer further containing "other structural units other than -[CH2C(CH3)2]- units". The component (A) preferably contains -[CH2C(CH3)2]- units in an amount of, for example, 70% by mass or more relative to the total amount of the structural units, preferably 75% by mass or more, and more preferably 80% by mass or more. In addition, the component (A) preferably contains -[CH2C(CH3)2]- units, for example, 100% by mass or less, in other embodiments, 95% by mass or less, and in other embodiments, 90% by mass or less. The component (A) preferably has 1 to 12 (meth)acryloyl groups, more preferably 2 to 8, further preferably 2 to 4, and particularly preferably 2. It should be noted that, in the present invention, the so-called polymer is not limited by theory but can be defined as, for example, a compound having a structure with a monomer repeating unit on the main chain of the polymer and containing more than 100 repeating units. In addition, the (meth)acryloyl group may be present in either the side chain and / or the terminal of the molecule, but is preferably present at the terminal of the molecule from the viewpoint of rubber elasticity.

[0040] As component (A), from the viewpoint of obtaining a curable resin composition having excellent cured product properties of high strength and high elongation, a polymer having a polyisobutylene skeleton represented by general formula (1) is preferred. As a specific example of component (A), polyisobutylene having a (meth)acryloyloxyalkoxyphenyl group can be cited. It should be noted that the main skeleton of component (A) in the present invention is a polyisobutylene skeleton. In addition to mainly using isobutylene as a monomer constituting the polyisobutylene skeleton, other monomers can also be used for copolymerization as long as the effect of the present invention is not impaired. It should be noted that since a curable resin composition that can cope with coating based on screen printing can be obtained, component (A) is further preferably in a liquid state at room temperature (25°C).

[0041] [Chemistry 2]

[0042]

[0043] In formula (1), R 1 It represents a monovalent or polyvalent aromatic hydrocarbon group, or a monovalent or polyvalent aliphatic hydrocarbon group which may have an aromatic ring. As the monovalent or polyvalent aromatic hydrocarbon group, an aryl group having 6 to 18 carbon atoms or an arylene group having 6 to 18 carbon atoms is preferred. Specific examples of the monovalent or polyvalent aromatic hydrocarbon group include phenyl, phenylene, naphthyl, naphthylene, biphenyl, tolyl, benzylidene, xylyl, xylylene, etc. As the monovalent or polyvalent aliphatic hydrocarbon group which may have an aromatic ring, it is an alkyl group having 6 to 18 carbon atoms, an alkylene group having 6 to 18 carbon atoms, an arylalkyl group having 6 to 18 carbon atoms, or an alkylene arylene alkylene group having 6 to 18 carbon atoms. Specific examples of monovalent or polyvalent aliphatic hydrocarbon groups which may have an aromatic ring include groups represented by -C(CH3)2CH2C(CH3)2CH3 group, -C(CH3)2CH2C(CH3)2CH2C(CH3)2- group, -C(CH3)2-C6H4-C(CH3)2- group (diisopropylphenyl group), etc. Among them, polyvalent aromatic hydrocarbon groups or aliphatic hydrocarbon groups which may have an aromatic ring are preferred, and bivalent groups are particularly preferred, such as preferably phenylene group and diisopropylphenyl group (more preferably p-diisopropylphenyl group).

[0044] PIB represents a polyisobutylene backbone containing -[CH2C(CH3)2]- units.

[0045] R 4It represents a divalent hydrocarbon group having 2 to 6 carbon atoms which may contain an oxygen atom, and is preferably a divalent hydrocarbon group having 2 or 3 carbon atoms. As the divalent saturated hydrocarbon group having 2 to 6 carbon atoms which may contain an oxygen atom, for example, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH2CH2-O-CH2CH2-, -CH2CH(OH)CH2-, etc. are preferred. Among them, -CH2CH2- is preferred.

[0046] R 2 and R 3 R each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably a hydrogen atom. 5 represents a hydrogen atom, a methyl group or an ethyl group, preferably a hydrogen atom or a methyl group. n is an integer of 1 to 6, and an integer of 2 to 4 is particularly preferred.

[0047] The molecular weight of the component (A) in the present invention is not particularly limited, but since it can cope with coating by screen printing and has excellent sealing properties, the number average molecular weight based on chromatography measurement is preferably, for example, 200 to 500000, more preferably 1000 to 100000, and particularly preferably 3000 to 50000. It should be noted that the number average molecular weight is calculated by the standard polystyrene conversion method using size permeation chromatography (SEC).

[0048] The viscosity of component (A) at 25°C in the present invention is not particularly limited, but from the perspective of workability, it is, for example, 5 Pa·s or more, preferably 50 Pa·s or more, more preferably 100 Pa·s or more, further preferably 500 Pa·s or more, and particularly preferably 1000 Pa·s or more; for example, 3000 Pa·s or less, preferably 2500 Pa·s or less, and more preferably 2000 Pa·s or less. The particularly preferred viscosity is 1800 Pa·s or less. It should be noted that, unless otherwise specified, the viscosity is measured using a cone-plate viscometer to measure the viscosity at 25°C.

[0049] The method for producing the component (A) is not particularly limited, but a known method can be used. For example, methods disclosed in Polymer Bulletin, Vol. 6, pp. 135-141 (1981), TPLiao and JPKennedy and Polymer Bulletin, Vol. 20, pp. 253-260 (1988), Puskas et al., which are obtained by reacting terminal hydroxy polyisobutylene with chlorinated acryloyl or chlorinated methacryloyl, etc. can be cited. In addition, as other methods for producing the component (A), methods for reacting terminal hydroxy polyisobutylene with a compound having a (meth) acryloyl group and an isocyanate group, methods for reacting terminal hydroxy polyisobutylene with a compound having an isocyanate group and a compound having a (meth) acryloyl group and a hydroxyl group, methods for reacting terminal hydroxy polyisobutylene with (meth) acrylic acid or (meth) acrylic acid lower ester using a dehydration esterification method or an ester exchange method, etc. can be cited.

[0050] In addition, the method for producing the polyisobutylene represented by the general formula (1) is not particularly limited, but a preferred method is a method disclosed in Japanese Patent Application Laid-Open No. 2013-216782 in which a halogen-terminated polyisobutylene is reacted with a compound having a (meth)acryloyl group and a phenoxy group as represented by the general formula (2). In addition, the halogen-terminated polyisobutylene can be obtained by a known method, for example, by cationic polymerization, more preferably by living cationic polymerization.

[0051] [Chemistry 3]

[0052]

[0053] In the general formula (2), R 2 , R 3 , R 4 , and R 5 It can be as described in the above general formula (1). Specifically, R 4 R represents a divalent hydrocarbon group having 2 to 6 carbon atoms which may contain an oxygen atom. 2 and R 3 R each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms. 5 represents a hydrogen atom, a methyl group, or an ethyl group. Examples of the compound represented by the general formula (2) include phenoxymethyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxybutyl (meth)acrylate, and phenoxypentyl (meth)acrylate, and preferably phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxybutyl (meth)acrylate, and phenoxypentyl (meth)acrylate.

[0054] <(B) Component>

[0055] The component (B) that can be used in the present invention is a radical polymerization initiator. As such a component (B), a photo radical polymerization initiator, an organic peroxide (thermal radical polymerization initiator), etc. can be cited. As for the cured form of the radical curable resin composition of the present invention, light curing, heat curing or redox curing can be selected by selecting the component (B) of the present invention. For example, when it is desired to impart "photocurability" to the radical curable resin composition, it is sufficient to select a photo radical polymerization initiator, and when it is desired to impart "curing based on heat curing or redox reaction", it is sufficient to select an organic peroxide.

[0056] The amount of the component (B) of the present invention is not particularly limited, but is, for example, 0.1 to 30 parts by mass, preferably 0.5 to 20 parts by mass, more preferably 0.3 to 18 parts by mass, further 1 to 15 parts by mass, and particularly preferably 1.5 to 10 parts by mass, relative to 100 parts by mass of the component (A). The amount of the component (B) within the above range is preferred from the viewpoint of being able to have high strength and high elongation properties of the cured product.

[0057] As one of the photo-radical polymerization initiators that can be used in the present invention (B) component, there is no particular limitation as long as it is a compound that generates free radicals by irradiating light (active energy rays). Here, active energy rays include radiation such as α rays, β rays, electromagnetic waves such as γ rays, X-rays, electron beams (EB), ultraviolet rays with a wavelength of about 100 to 400 nm, visible light with a wavelength of about 400 to 800 nm, and all of the broad light, preferably ultraviolet rays. As for the photo-radical polymerization initiator as the (B) component, for example, acetophenone-based photo-radical polymerization initiators, benzoin-based photo-radical polymerization initiators, benzophenone-based photo-radical polymerization initiators, thioxanthone-based photo-radical polymerization initiators, acylphosphine oxide-based photo-radical polymerization initiators, titanocene-based photo-radical polymerization initiators, etc., among which, from the viewpoint of obtaining a high-strength, high-elongation cured product, acetophenone-based photo-radical polymerization initiators and acylphosphine oxide-based photo-radical polymerization initiators are preferred. In addition, they can be used alone or in combination of two or more.

[0058] Examples of the acetophenone-based photoradical polymerization initiator include, but are not limited to, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, benzyl dimethyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-methyl-2-morpholino(4-thiomethylphenyl)propane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, and 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone oligomers. Examples of commercially available acetophenone-based photoradical polymerization initiators include Omnirad (registered trademark, hereinafter the same) 184, Omnirad 1173, Omnirad 2959, Omnirad 127, and ESACURE (registered trademark) KIP-150 (manufactured by IGM Resins BV).

[0059] As the acylphosphine oxide-based photoradical polymerization initiator, for example, bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc. can be mentioned, but it is not limited thereto. As commercial products of the acylphosphine oxide-based photoradical polymerization initiator, Omnirad TPO, Omnirad 819, Omnirad 819DW (manufactured by IGM Resins BV) can be mentioned.

[0060] The organic peroxide, which is one of the components (B) that can be used in the present invention, is a compound that generates free radical species by heating or redox reaction. Here, the heating is preferably a temperature of 50°C or more, preferably a temperature of 80°C or more, and more preferably a temperature of 100°C or more. The compound that generates free radical species by heating is also particularly called a thermal free radical polymerization initiator. Redox reaction is also called redox reaction, which is a phenomenon that a redox reaction is caused by free radical species released by the organic peroxide. If redox reaction is used, free radical species can be generated at room temperature, so it is preferred.The organic peroxide as component (B) is not particularly limited, and examples thereof include ketone peroxides such as methyl ethyl ketone peroxide, cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, methylcyclohexanone peroxide, methyl acetoacetate peroxide, and acetylacetone peroxide; peroxyketals such as 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)octane, n-butyl-4,4-bis(tert-butylperoxy)valerate, and 2,2-bis(tert-butylperoxy)butane; tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, p-menthane; Hydrogen peroxides such as hydrogen peroxide, 2,5-dimethylhexane-2,5-dihydroperoxide, and 1,1,3,3-tetramethylbutyl hydroperoxide; dialkyl peroxides such as di-tert-butyl peroxide, tert-butyl isopropyl peroxide, diisopropyl benzene peroxide, α,α'-bis(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; acetyl peroxide, isobutyryl peroxide, octanoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 3,5,5-trimethylhexanoyl peroxide diacyl peroxides such as succinic acid peroxide, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, m-toluoyl peroxide; diisopropyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-n-propyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, dimyristyl peroxydicarbonate, di(2-ethoxyethyl) peroxydicarbonate, dimethoxyisopropyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, diallyl peroxydicarbonate, etc.; tert-butyl peroxyacetate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, Oxidized tert-butyl neodecanoate, peroxy neodecanoic acid cumyl ester, peroxy-2-ethylhexanoic acid tert-butyl ester, peroxy-3,5,5-trimethylhexanoic acid tert-butyl ester, peroxy laurate tert-butyl ester, peroxy benzoate tert-butyl peroxide, peroxy isophthalic acid di-tert-butyl ester, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, peroxy maleic acid tert-butyl ester, peroxy isopropyl carbonate tert-butyl ester, peroxy octanoic acid cumyl ester, peroxy neodecanoic acid tert-hexyl ester, peroxy pivalic acid tert-butyl peroxide, peroxy neohexanoic acid tert-hexyl ester, peroxy neohexanoic acid cumyl ester and other peroxyesters; and acetyl cyclohexyl sulfonyl peroxide, peroxy allyl carbonate tert-butyl ester, etc. These organic peroxides can be used alone or in combination. Among them, from the viewpoint of high strength and high elongation cured product properties, cumene hydroperoxide is preferably used.

[0061] When an organic peroxide is used as component (B), a curing accelerator may be added for the purpose of promoting the redox reaction. Such a curing accelerator is not particularly limited, but preferably saccharin (o-benzoylsulfonyl imide), a hydrazine compound, an amine compound, a thiol compound, a transition metal-containing compound, etc. are used.

[0062] Examples of the hydrazine compound include 1-acetyl-2-phenylhydrazine, 1-acetyl-2 (p-tolyl) hydrazine, 1-benzoyl-2-phenylhydrazine, 1-(1',1',1'-trifluoro)acetyl-2-phenylhydrazine, 1,5-diphenyl-carbohydrazide, 1-formyl-2-phenylhydrazine, 1-acetyl-2-(p-bromophenyl) hydrazine, 1-acetyl-2-(p-nitrophenyl) hydrazine, 1-acetyl-2-(2'-phenylethylhydrazine), ethyl carbazate, p-nitrophenylhydrazine, and p-trisulfonylhydrazide.

[0063] Examples of the amine compound include heterocyclic secondary amines such as 2-ethylhexylamine, 1,2,3,4-tetrahydroquinone, and 1,2,3,4-tetrahydroquinaldine; heterocyclic quaternary amines such as quinoline, methylquinoline, quinaldine, and quinoxalinephenazine; aromatic quaternary amines such as N,N-dimethyl-p-toluidine, N,N-dimethyl-anisidine, and N,N-dimethylaniline; and azole compounds such as 1,2,4-triazole, oxazole, oxadiazole, thiadiazole, benzotriazole, hydroxybenzotriazole, benzoxazole, 1,2,3-benzothiadiazole, and 3-mercaptobenzotriazole.

[0064] Examples of the thiol compound include n-dodecyl mercaptan, ethyl mercaptan, butyl mercaptan, tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexa(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane trimercaptoacetate, and pentaerythritol tetrakismercaptoacetate.

[0065] As the transition metal-containing compound, a metal chelate complex is preferably contained, for example, iron pentanedione, cobalt pentanedione, copper pentanedione, copper propylenediamine, copper ethylenediamine, iron naphthenate, nickel naphthenate, cobalt naphthenate, copper naphthenate, copper octanoate, iron hexanoate, iron propionate, vanadium acetylacetonate, etc. can be cited.

[0066] The above-mentioned curing accelerators may be used alone or in combination of two or more thereof. Among them, saccharin, hydrazine compounds, amine compounds, and mixtures of transition metal-containing compounds are more preferred because they exhibit good curing accelerating effects.

[0067] <(C) Ingredients>

[0068] The component (C) of the present invention is a defoamer containing a silicone compound without a methoxysilyl group, an ethoxysilyl group, and a (meth)acryloyl group and containing no organic solvent. That is, the defoamer does not contain an organic solvent and contains a silicone compound without a methoxysilyl group, an ethoxysilyl group, and a (meth)acryloyl group. The present invention has the following significant effect, and can select the component (C) of the present invention from a large number of defoamers and combine it with other components of the present invention, thereby maintaining the high strength and high elongation properties of the cured product while coping with a curable resin composition based on screen printing coating. The above-mentioned silicone compound can include compounds containing -Si-O-Si- (siloxane bond), and more specifically, compounds having structures such as dimethylsiloxane, methylphenylsiloxane, and diphenylsiloxane. In addition, as for the silicone compound of the component (C), from the viewpoint of small repulsion when the curable resin composition is applied to the adherend by screen printing while maintaining the tensile strength of the cured product, it is a compound that does not have a methoxysilyl group, an ethoxysilyl group, and a (meth)acryloyl group at the end or side chain of one molecule of the silicone compound, and preferably a compound in which at least one of the ends is blocked by a trimethylsilyl group. In addition, as for the component (C), from the viewpoint of small repulsion when the curable resin composition is applied to the adherend by screen printing while maintaining the tensile strength of the cured product, it is characterized in that it does not contain an organic solvent. Here, in this specification, an organic solvent refers to an organic compound that is liquid at 25°C other than the silicone compound, the component (B), and the component (D), for example, propylene glycol, diisobutyl ketone, etc. can be cited. In addition, as described later, the curable resin composition of the present invention preferably does not contain an organic solvent, and for this reason, the component (C) does not contain an organic solvent.

[0069] The silicone compound contained in the component (C) preferably contains a dimethylpolysiloxane structure having a siloxane bond (Si-O-Si) and a methyl group. When the silicone compound contained in the component (C) contains a dimethylpolysiloxane structure, the desired effect of the present invention can be better exerted, and a curable resin composition suitable for screen printing can be obtained.

[0070] The silicone compound contained in the component (C) is preferably a silicone oil which is one kind of silicone compound. Therefore, the component (C) is preferably an oil-type defoaming agent.

[0071] The silicone compound contained in the component (C) preferably has a viscosity of 1 to 500 mm at 25°C. 2 / s, more preferably 10 to 350 mm 2By setting the viscosity of the silicone compound at 25°C to the above range, the effect as a defoamer can be properly exerted. In addition, from the viewpoint of exerting the effect of the defoamer, the viscosity of the component (C) at 25°C is preferably 1 to 500 mm / s. 2 / s, more preferably 10 to 350 mm 2 / s range.

[0072] In component (C), a silicone compound is preferably contained as a main component. In this specification, the main component refers to 75% by mass or more relative to the total mass of component (C). In addition, in component (C), the upper limit of the content of the silicone compound is 100% by mass relative to the total mass of component (C). The content of the silicone compound in component (C) is preferably 80% by mass or more relative to the total mass of the defoamer, more preferably 90% by mass or more, and further preferably 95% by mass or more.

[0073] (C) component may contain additives within the range that does not damage the characteristics of the defoamer. As additives, waxes such as polyethylene wax, hydrophobic silica, etc. can be cited. For example, the content of the additive in the (C) component is 25% by mass or less, preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, and particularly preferably 5% by mass or less. The lower limit of the content of the additive in the (C) component is 0% by mass relative to the total mass of the (C) component.

[0074] Examples of commercially available products of the component (C) of the present invention include BYK-1799 (manufactured by BYK-Chemie) and KF-96 series (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0075] There is no particular restriction on the amount of (C) added, but for example, relative to 100 parts by mass of the (A) component, the content of the (C) component is in the range of 0.1 to 10 parts by mass, preferably in the range of 0.15 to 5 parts by mass, more preferably in the range of 0.15 to 4.5 parts by mass, further preferably in the range of 0.2 to 4 parts by mass, particularly preferably in the range of 0.2 to 3 parts by mass, and further preferably in the range of 0.5 to 2.5 parts by mass. In addition, relative to 100 parts by mass of the total amount of the (A) component and the (D) component described later, the content of the (C) component is preferably in the range of 0.1 to 9 parts by mass, more preferably in the range of 0.2 to 7 parts by mass, further preferably in the range of 0.3 to 5 parts by mass, particularly preferably in the range of 0.3 to 3 parts by mass, and most preferably in the range of 0.3 to 1.5 parts by mass. By being within the above range, a curable resin composition that can cope with coating based on screen printing while maintaining high strength and high elongation cured product properties can be obtained.

[0076] <(D) Component>

[0077] Furthermore, the curable resin composition of the present invention can further contain a monofunctional monomer as the (D) component. The (D) component can be further adapted to coating based on screen printing and maintain the properties of the cured product by combining with other components (components ((A) to (C)) of the present invention. As the (D) component, for example, a (meth)acrylate monomer having an alkyl group with 5 to 30 carbon atoms or a (meth)acrylate monomer having an alicyclic hydrocarbon group with 5 to 30 carbon atoms can be cited. Among them, from the viewpoint of being able to further cope with coating based on screen printing and maintaining the properties of the cured product, it is particularly preferred to use a (meth)acrylate monomer having an alkyl group with 5 to 30 carbon atoms and a (meth)acrylate monomer having an alicyclic hydrocarbon group with 5 to 30 carbon atoms in combination.

[0078] Examples of the (meth)acrylate monomer having an alkyl group with 5 to 30 carbon atoms include 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, n-octadecyl (meth)acrylate, isooctyl (meth)acrylate, nonadecyl (meth)acrylate, isostearyl (meth)acrylate, and stearyl (meth)acrylate. Among them, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isooctyl (meth)acrylate, isostearyl (meth)acrylate, and stearyl (meth)acrylate are preferred. Among the (meth)acrylate monomers having an alkyl group with 5 to 30 carbon atoms, those having an alkyl group with 6 to 20 carbon atoms are preferred, and those having an alkyl group with 8 to 20 carbon atoms are preferred. Component (D) can be used alone or as a mixture of two or more. Commercially available products of (meth)acrylate monomers having an alkyl group with 5 to 30 carbon atoms are not particularly limited, but examples thereof include SR335, SR395, SR440, SR489D, SR313, SR324, SR493D (manufactured by Sartomer Co., Ltd.), and S-1800A (manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0079] In addition, examples of (meth)acrylate monomers having an alicyclic hydrocarbon group having 5 to 30 carbon atoms include cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, dicyclopentyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, and dicyclopentenyl di(meth)acrylate. Among them, trimethylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, dicyclopentyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, and isobornyl (meth)acrylate are preferred. These may be used alone or as a mixture of two or more. Among the (meth)acrylate monomers having an alicyclic hydrocarbon group having 5 to 30 carbon atoms, those having an alicyclic hydrocarbon group having 6 to 20 carbon atoms are preferred, and those having an alicyclic hydrocarbon group having 8 to 20 carbon atoms are preferred. Commercially available products of the (meth)acrylate monomers having an alicyclic hydrocarbon group having 5 to 30 carbon atoms are not particularly limited, but examples thereof include SR506, SR423 (produced by Sartomer), IBX, IBX-A (produced by Kyoeisha Chemical Co., Ltd.), FA-511AS, FA-512AS, FA-513AS, FA-512M, FA-512MT, and FA-513M (produced by Showa Denko Materials Co., Ltd.).

[0080] The amount of component (D) is preferably 5 to 500 parts by mass, more preferably 10 to 300 parts by mass, further preferably 12 to 200 parts by mass, particularly preferably 30 to 150 parts by mass, and most preferably 40 to 100 parts by mass, relative to 100 parts by mass of component (A). Within the above range, a curable resin composition that can cope with coating based on screen printing and can be photocured in a short time can be further provided. It should be noted that when two or more components (D) are combined, the total amount thereof is taken as the content of component (D). In addition, when a (meth)acrylate monomer having an alkyl group having 5 to 30 carbon atoms and a (meth)acrylate monomer having an alicyclic hydrocarbon group having 5 to 30 carbon atoms are used in combination, the mass ratio (x:y) of the (meth)acrylate monomer having an alkyl group having 5 to 30 carbon atoms (x) and the (meth)acrylate monomer having an alicyclic hydrocarbon group having 5 to 30 carbon atoms (y) is, for example, in the range of 1:99 to 99:1, preferably in the range of 10:90 to 90:10, and particularly preferably in the range of 15:85 to 85:15.

[0081] <Optional Ingredients>

[0082] To the curable resin composition of the present invention, additives such as an oligomer or polymer having a (meth)acryloyl group (not including the component (A) of the present invention), an inorganic filler, a curing accelerator, a storage stabilizer, an antioxidant, a light stabilizer, a plasticizer, a pigment, a flame retardant, and a surfactant may be added within a range that does not impair the purpose of the present invention.

[0083] The oligomer or polymer having a (meth)acryloyl group (excluding the component (A) of the present invention) is not particularly limited, and examples thereof include polybutadiene skeleton urethane (meth)acrylates, hydrogenated polybutadiene skeleton urethane (meth)acrylates, polycarbonate skeleton urethane (meth)acrylates, polyether skeleton urethane (meth)acrylates, polyester skeleton urethane (meth)acrylates, castor oil skeleton urethane (meth)acrylates, isoprene skeleton (meth)acrylates, (meth)acrylate, hydrogenated isoprene (meth)acrylate, epoxy (meth)acrylate, (meth)acryloyl-containing acrylic polymer, etc. Among them, polybutadiene skeleton urethane (meth)acrylate, hydrogenated polybutadiene skeleton urethane (meth)acrylate, castor oil skeleton urethane (meth)acrylate, isoprene (meth)acrylate, hydrogenated isoprene (meth)acrylate are preferred due to their excellent compatibility with the components (A) and (B) of the present invention. It should be noted that in the present invention, the oligomer refers to a compound having a structure with a repeating unit of a monomer in the main chain and containing 2 to 100 repeating units. In addition, they can be used alone or in combination of two or more.

[0084] For the curable resin composition of the present invention, for the purpose of improving the elastic modulus, fluidity, etc. of the cured product, an inorganic filler can be added to a degree that does not damage the storage stability. Specifically, inorganic powders, metallic powders, etc. can be cited. As fillers for inorganic powders, glass, fumed silica, alumina, mica, ceramics, silicone rubber powder, calcium carbonate, aluminum nitride, carbon powder, kaolin clay, dry clay minerals, dry diatomaceous earth, etc. can be cited. The amount of inorganic powder is preferably about 0.1 to 100 parts by mass relative to 100 parts by mass of component (A).

[0085] For the purpose of adjusting the viscosity of curable resin composition or improving the mechanical strength of cured product, fumed silica can be coordinated. Fumed silica etc. that hydrophobic treatment is carried out with organochlorosilanes, polyorganosiloxane, hexamethyldisilazane etc. can be preferably used. As the specific example of fumed silica, for example, the commercially available products such as trade name Aerosil (registered trademark) R974, R972, R972V, R972CF, R805, R812, R812S, R816, R8200, RY200, RX200, RY200S, R202 etc. made by Japan Aerosil can be enumerated.

[0086] An antioxidant may be added to the curable resin composition of the present invention. Examples of the antioxidant include quinone compounds such as β-naphthoquinone, 2-methoxy-1,4-naphthoquinone, methyl hydroquinone, hydroquinone, hydroquinone monomethyl ether, mono-tert-butyl hydroquinone, 2,5-di-tert-butyl hydroquinone, p-benzoquinone, 2,5-diphenyl-p-benzoquinone, and 2,5-di-tert-butyl-p-benzoquinone; phenothiazine, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), catechol, tert-butylcatechol, 2-butyl-4-hydroxyanisole, 2,6-di-tert-butyl-p-cresol, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl 〕-4,6-di-tert-pentylphenyl acrylate, 4,4'-butylenebis(6-tert-butyl-3-methylphenol), 4,4'-thiobis(6-tert-butyl-3-methylphenol), 3,9-bis[2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, pentaerythritol tetra[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-hexane-1,6-diylbis[3- (3,5-di-tert-butyl-4-hydroxyphenyl) propionamide, phenylpropionic acid, 3,5-bis(1,1-dimethylethyl)-4-hydroxy-C7-C9 side chain alkyl ester, 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl 〔〔3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl〕methyl〕phosphonate, 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6-tolyl)tri-p-cresol, diethyl bis〔〔3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl〕methyl〕phosphonate calcium, 4,6-bis(octylthiomethyl)-o-cresol, ethylenebis(oxyethylene)bis〔3-(5-tert-butyl)- Phenolic compounds such as 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-xylyl)methyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, reaction product of N-phenylaniline and 2,4,6-trimethylpentene, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazine-2-ylamino)phenol, picric acid, citric acid, etc.Tris(2,4-di-tert-butylphenyl)phosphite, tris[2-[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphin-6-yl][oxy][ethyl]amine, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl phosphite, tetrakis(2,4-di-tert-butylphenyl)[1,1-biphenyl]-4,4'-diylbisphosphonite, 6-[3-(3- Phosphorus compounds such as tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphine (phosphepin); sulfur compounds such as dilauryl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythritol tetrakis (3-laurylthiopropionate), 2-mercaptobenzimidazole; amine compounds such as phenothiazine; lactone compounds; vitamin E compounds, etc. Among them, phenol compounds are preferred. ;

[0087] A light stabilizer may be added to the curable resin composition of the present invention. Examples of the light stabilizer include bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 1-[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]-2,2,6,6-tetramethylpiperidine, 1,2,2,6,6-pentamethyl-4-piperidinyl-methacrylate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methacrylate. 1,10-diamine, dibutylamine, 1,3,5-triazine, N,N'-bis(2,2,6,6-tetramethyl-1(octyloxy)-4-piperidinyl) sebacate, reaction product of 1,1-dimethylethyl hydroperoxide and octane, N,N',N",N"'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine, polycondensation product of dibutylamine, 1,3,5-triazine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidinyl)butylamine, poly[[6-(1,1,3,3-tetramethylbutyl] )amino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino][hexamethylene][(2,2,6,6-tetramethyl-4-piperidinyl)imino][], polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol, 2,2,4,4-tetramethyl-20-(β-lauryloxycarbonyl)ethyl-7-oxa-3,20-diazabispiperidin-21-one, β-alanine, N,-(2,2,6,6-tetramethyl-4-piperidinyl)-dodecyl ester / tetradecyl ester, N-acetyl-3-dodecyl-1-(2,2,6,6-tetramethyl hindered amine compounds such as 2,2,4,4-tetramethyl-7-oxa-3,20-diazabispiro〔5,1,11,2〕heneicosane-21-one, 2,2,4,4-tetramethyl-21-oxa-3,20-diazabicyclo-〔5,1,11,2〕heneicosane-20-propionic acid dodecyl ester / tetradecyl ester, malonic acid,〔(4-methoxyphenyl)-methylene〕-bis(1,2,2,6,6-pentamethyl-4-piperidyl) ester, higher fatty acid esters of 2,2,6,6-tetramethyl-4-piperidinol, 1,3-benzenedicarboxylic acid amide, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl);Octabenzone and other benzophenone compounds; 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-〔2-hydroxy-3-(3,4,5,6-tetrahydrophthalimide-methyl)-5-methylphenyl〕benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-pentylphenyl) Benzotriazole, a reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl) propionate and polyethylene glycol, 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol and other benzotriazole compounds; 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate and other benzoate compounds; 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-〔(hexyl)oxy〕phenol and other triazine compounds, etc. Hindered amine compounds are particularly preferred. ;

[0088] The curable resin composition of the present invention may be added with a close-fitting agent. Examples of the close-fitting agent include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, methacryloxyoctyltrimethoxysilane, vinyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyl-tri(β-methoxyethoxy)silane, γ-chloropropyltrimethoxysilane, β-(3,4-epoxy)silane, 1,2-dimethoxy- ... cyclohexyl)ethyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-mercaptopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-ureidopropyl triethoxysilane, hydroxyethyl methacrylate phosphate, methacryloyloxyoxyethyl acid phosphate, methacryloyloxyoxyethyl acid phosphate monoethylamine half salt, 2-hydroxyethyl methacrylate phosphate, etc. Among them, hydroxyethyl methacrylate phosphate, methacryloyloxyoxyethyl acid phosphate, methacryloyloxyoxyethyl acid phosphate monoethylamine half salt, 2-hydroxyethyl methacrylate phosphate, etc. are preferred. The content of the adhesion-imparting agent is preferably 0.05 to 30 parts by mass, and more preferably 0.2 to 10 parts by mass, relative to 100 parts by mass of the component (A).

[0089] The curable resin composition of the present invention preferably does not contain an organic solvent from the viewpoint of maintaining the tensile strength of the cured product while minimizing repulsion when the curable resin composition is applied to an adherend by screen printing. The organic solvent refers to an organic compound that is liquid at 25° C. other than the silicone compound, component (B), component (C) and component (D), and examples thereof include propylene glycol and diisobutyl ketone.

[0090] The viscosity of the curable resin composition of the present invention at 25°C is not particularly limited, but from the perspective of workability, it is, for example, 0.1 Pa·s or more, preferably 0.2 Pa·s or more, more preferably 0.5 Pa·s or more, further preferably 1 Pa·s or more, particularly preferably 2 Pa·s or more, for example 100 Pa·s or less, preferably 50 Pa·s or less, more preferably 20 Pa·s or less. The particularly preferred viscosity is 10 Pa·s or less. It should be noted that, unless otherwise specified, the viscosity is measured using a cone-plate viscometer to measure the viscosity at 25°C.

[0091] The curable resin composition of the present invention can be produced by a conventionally known method. For example, it can be produced by mixing the predetermined amounts of components (A) to (C) using a mixing means such as a mixer at a temperature of preferably 10 to 70° C. for preferably 0.1 to 5 hours. In addition, it is preferably produced under a light-shielding environment.

[0092] <Coating method>

[0093] As a method for applying the curable resin composition of the present invention to an adherend, for example, dispensing, spraying, inkjetting, screen printing, gravure printing, dipping, spin coating, etc. using an automatic coating machine can be used. Among them, the curable resin composition of the present invention is most suitable for screen printing because it can exert the effect of defoaming the bubbles generated during screen printing. It should be noted that from the viewpoint of coating properties, the curable resin composition of the present invention is preferably in a liquid state at 25°C.

[0094] <Curing method>

[0095] The light source for curing the curable resin composition of the present invention by irradiating light such as ultraviolet rays and visible light is not particularly limited, and examples thereof include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, black light lamps, microwave-excited mercury lamps, metal halide lamps, sodium lamps, halogen lamps, xenon lamps, LEDs, fluorescent lamps, sunlight, electron beam irradiation devices, and the like. From the viewpoint of the properties of the cured product, the irradiation dose of light irradiation is preferably 3 kJ / m 2 More preferably 5 kJ / m 2 From the perspective of the production cycle time of the curing process, 100 kJ / m 2Below, more preferably 80 kJ / m 2 Below, particularly preferably 60 kJ / m 2 the following.

[0096] <Cured product>

[0097] The cured product of the present invention is obtained by curing the curable resin composition of the present invention by irradiating ultraviolet rays using the above-mentioned curing method. The cured product of the present invention may be cured by any method as long as it is a cured product obtained by curing the curable resin composition of the present invention.

[0098] <Application and sealant>

[0099] As a suitable application for the curable resin composition of the present invention or its cured product, a curable sealant is used. In the present invention, the sealant also includes applications such as adhesives, coating agents, casting agents, potting agents, etc. It should be noted that when used in such applications, the curable resin composition of the present invention is preferably liquid at 25°C.

[0100] The curable resin composition of the present invention or its cured product is a rubber elastic body having excellent low gas permeability (gas barrier property), low moisture permeability, heat resistance, acid resistance, flexibility, etc. Therefore, as specific uses of the sealant, fuel cells, solar cells, dye-sensitized solar cells, lithium-ion batteries, electrolytic capacitors, liquid crystal displays, organic EL displays, electronic paper, LEDs, hard disk devices, photodiodes, optical communication circuits, wires, cables, optical fibers, optical isolators, IC cards and other laminates, sensors, substrates, pharmaceuticals, medical instruments, equipment, etc. The curable resin composition of the present invention is rapidly cured by irradiation with active energy rays such as ultraviolet rays and has excellent gas barrier properties, so among these uses, fuel cell use is particularly preferred.

[0101] <Fuel Cell>

[0102] A fuel cell is a power generation device that generates electricity by chemically reacting hydrogen and oxygen. In addition, fuel cells include four types: solid polymer fuel cells, phosphoric acid fuel cells, molten carbonate fuel cells, and solid oxide fuel cells. Among them, solid polymer fuel cells are used for automotive power sources, household power generation devices, small power sources for electronic devices such as mobile phones, emergency power sources, etc. due to their relatively low operating temperature (around 80°C) and high power generation efficiency.

[0103] like Figure 1As shown, a representative solid polymer fuel cell battery unit 1 is a structure having an electrolyte membrane electrode assembly 5 (MEA), a frame 6 supporting the MEA, and a diaphragm 2 forming a gas flow path, wherein the electrolyte membrane electrode assembly 5 (MEA) is a structure in which a polymer electrolyte membrane 4 is clamped between an air electrode 3a and a fuel electrode 3b. In addition, when the solid polymer fuel cell is started, fuel gas (hydrogen) and oxidizing gas (oxygen) are supplied through the oxidizing gas flow path 8a and the fuel gas flow path 8b. In addition, in order to alleviate the heat generated during power generation, cooling water flows through the flow path 9. It should be noted that, as Figure 2 As shown, a device in which several hundred battery cells are stacked and packaged is called a battery pack 10 .

[0104] If fuel gas (hydrogen) is supplied to the fuel electrode and oxidizing gas (oxygen) is supplied to the oxygen electrode (air electrode), the following reaction occurs at each electrode, and a reaction to generate water occurs as a whole (H2+1 / 2O2→H2O). In detail, as described below, the protons (H+) generated in the fuel electrode diffuse in the solid polymer membrane and move to the oxygen electrode side, and the water (H2O) generated by the reaction with oxygen is discharged from the oxygen electrode side.

[0105] Fuel electrode (anode): H2→2H+ + 2e -

[0106] Oxygen electrode (cathode): 1 / 2O2+2H + +2e - →H2O

[0107] In order to start a solid polymer fuel cell, it is necessary to supply a fuel gas containing hydrogen to the anode and an oxidizing gas containing oxygen to the cathode in a separately isolated manner. This is because there is a risk that if the isolation is insufficient and the gas on one side is mixed with the gas on the other side, it may cause a decrease in power generation efficiency. Based on this background, sealants are mostly used for the purpose of preventing leakage of fuel gas, oxygen, etc. Specifically, sealants are used between adjacent diaphragms, between diaphragms and frames, between frames and electrolyte membranes or MEA, etc.

[0108] As the aforementioned polymer electrolyte membrane, a cation exchange membrane with ion conductivity can be cited, and from the aspect of making the chemically stable and high temperature working strong, preferably a fluorine-based polymer with a sulfonic acid group can be cited. As a commercially available product, Nafion (registered trademark) made by DuPont, FLEMION (registered trademark) made by AGC Co., Ltd., Aciplex (registered trademark) made by Asahi Kasei Co., Ltd., etc. can be cited. Usually, the polymer electrolyte membrane is a material that is difficult to bond, but can be bonded by using the curable resin composition of the present invention.

[0109] [Chemistry 4]

[0110]

[0111] Nafion(Registered Trademark)

[0112] The above-mentioned fuel electrode is called a hydrogen electrode or an anode, and a known electrode can be used. For example, an electrode formed by supporting a catalyst such as platinum, nickel, or ruthenium on carbon can be used. In addition, the above-mentioned air electrode is called an oxygen electrode or a cathode, and a known electrode can be used. For example, an electrode formed by supporting a catalyst such as platinum or an alloy on carbon can be used. The surface of each electrode can be provided with a gas diffusion layer having the function of promoting the diffusion of gas and the moisturizing of electrolyte. A known gas diffusion layer can be used for the gas diffusion layer, but for example, carbon paper, carbon cloth, carbon fiber, etc. can be cited.

[0113] like Figure 1 As shown, the separator 2 has a concave and convex fine flow path, and the fuel gas and the oxidizing gas are supplied to the electrode through the flow path. In addition, the separator is made of aluminum, stainless steel, titanium, graphite, carbon, etc.

[0114] The frame is supported and reinforced in a way that the thin film electrolyte membrane or MEA will not break. As the material of the frame, thermoplastic resins such as polyvinyl chloride, polyethylene naphthalate, polyethylene terephthalate, polypropylene, and polycarbonate can be cited. In addition, in order to use the curable resin composition of the present invention or its cured product to bond components, the frame is preferably made of a light-transmitting material.

[0115] The fuel cell of the present invention is a fuel cell characterized by being sealed by the curable resin composition of the present invention or its cured product. As components that need to be sealed in the fuel cell, diaphragms, frames, electrolyte membranes, fuel electrodes, air electrodes, MEA, etc. can be cited. As more specific sealing parts, adjacent diaphragms, diaphragms and frames, frames and electrolyte membranes or MEA, etc. can be cited. It should be noted that the main purpose of sealing "between diaphragms and frames" or "between polymer electrolyte membranes or MEA and frames" is to prevent gas mixing and leakage, and the purpose of sealing between adjacent diaphragms is to prevent gas leakage and prevent cooling water from leaking from the cooling water flow path to the outside. It should be noted that, because the acid generated by the electrolyte membrane becomes a strong acid atmosphere, acid resistance is required for the sealant.

[0116] <Sealing method>

[0117] The sealing method using the curable resin composition of the present invention is not particularly limited, but typical examples include FIPG (formed in place gasket), CIPG (cured in place gasket), MIPG (molded in place gasket), liquid injection molding, and the like.

[0118] FIPG is a method in which the curable resin composition of the present invention is applied to the flange of the sealed component by an automatic coating device or the like, and in a state where the flange is bonded to another flange, active energy rays such as ultraviolet rays are irradiated from the light-transmissive flange side to cure the curable resin composition and perform adhesive sealing. More specifically, a sealing method is a method for sealing at least a portion between the at least two flanges of a sealed component having at least two flanges, characterized in that at least one of the flanges is permeable to active energy rays, and the method comprises: a step of applying the curable resin composition to the surface of at least one of the flanges; a step of bonding one flange (coated surface) coated with the curable resin composition and another flange with the curable resin composition interposed therebetween; and a step of irradiating the flange permeable to active energy rays to cure the curable resin composition and thereby sealing at least a portion between the at least two flanges.

[0119] CIPG is a method in which the curable resin composition of the present invention is applied to the flange of the sealed component in the form of beads by using a screen printing coating device, an automatic coating device, etc., and active energy rays such as ultraviolet rays are irradiated to cure the curable resin composition to form a gasket, which is then bonded to another flange for compression sealing. More specifically, a sealing method is a method for sealing at least a portion between the at least two flanges of a sealed component having at least two flanges, characterized in that it includes: a step of applying the curable resin composition to at least one flange; a step of irradiating the applied curable resin composition with active energy rays to cure the curable resin composition to form a gasket composed of a cured product of the curable resin composition; and a step of arranging another flange on the gasket, and pressing the one flange coated with the curable resin composition and the other flange with the gasket sandwiched therebetween to seal at least a portion between the at least two flanges.

[0120] MIPG is a method in which a mold is pre-crimped to the flange of a component to be sealed, a curable resin composition is injected into the cavity formed between the mold made of a light-transmissive material and the flange, and active energy rays such as ultraviolet rays are irradiated to cause photocuring to form a gasket. Then, it is bonded to another flange and compression-sealed. It should be noted that the mold is preferably made of a light-transmissive material. Specifically, glass, polymethyl methacrylate (PMMA), polycarbonate, cycloolefin polymer, olefin, etc. can be cited. In addition, in order to easily remove the mold after forming the gasket, the mold is preferably pre-coated with a release agent such as a fluorine-based or silicone-based one. More specifically, a sealing method for sealing at least a part between at least two flanges of a component to be sealed having at least two flanges, characterized by comprising: a step of disposing a mold for forming a gasket on at least one of the above flanges; a step of injecting at least a part of the above curable resin composition into the gap between the above gasket-forming mold and the above one flange on which the mold is disposed; a step of irradiating the above curable resin composition with the above active energy rays to cure the above curable resin composition to form a gasket composed of a cured product of the above curable resin composition; a step of removing the above mold from the above one flange; and a step of disposing another flange on the above gasket and crimping the above one flange and the above another flange with the above gasket interposed therebetween to seal at least a part between the above at least two flanges.

[0121] Liquid injection molding is a method in which the curable resin composition of the present invention is flowed into a mold made of a light-transmissive material under a specific pressure, and active energy rays such as ultraviolet rays are irradiated to cause photocuring to form a gasket. In addition, it is a method of bonding to another flange and performing compression sealing. It should be noted that the mold is preferably made of a light-transmissive material. Specifically, glass, PMMA, polycarbonate, cycloolefin polymer, olefin, etc. can be cited. In addition, in order to easily remove the mold after forming the gasket, it is preferable to pre-coat the mold with a release agent such as a fluorine-based or silicone-based one.

[0122] Examples

[0123] Examples are given below to explain the present invention in more detail. The present invention is not limited to these examples.

[0124] <Manufacture of a1>

[0125] Manufacture of polyisobutene (a1) having acryloyloxyethoxyphenyl

[0126] After nitrogen substitution in a 5L separable flask, 200mL of n-hexane and 2000mL of chlorobutane were added, and the mixture was cooled to -70°C while stirring under a nitrogen atmosphere. Next, 840mL (9mol) of isobutylene, 12g (0.05mol) of p-diisopropylbenzene chloride, and 1.1g (0.012mol) of 2-methylpyridine were added. After the reaction mixture was cooled to -70°C, 5.0mL (0.05mol) of titanium tetrachloride was added to initiate polymerization. Three hours after the start of the polymerization, 40g of phenoxyethyl acrylate (LIGHT ACRYLATE PO-A, manufactured by Kyoeisha Chemical Co., Ltd.) and 110ml of titanium tetrachloride were added. Subsequently, stirring was continued at -70°C for 4 hours, and then 1000ml of methanol was added to stop the reaction.

[0127] The supernatant was separated from the reaction solution, and the solvent was distilled off. The product was then dissolved in 3000 ml of n-hexane and washed three times with 3000 ml of pure water. After reprecipitation from methanol, the solvent was distilled off under reduced pressure, and the obtained polymer was vacuum dried at 80°C for 24 hours to obtain polyisobutylene (a1) having acryloyloxyethoxyphenyl group.

[0128] The above-mentioned a1 contains a -[CH2C(CH3)2]- unit and contains two acryloyl groups. More specifically, a1 is R 1 is diisopropylphenyl, PIB is a polyisobutylene skeleton, R 4 is a hydrocarbon group having 2 carbon atoms, R 2 and R 3 Each independently represents a hydrogen atom, R 5 It is a polymer of hydrogen atoms. The number average molecular weight (chromatographic method, polystyrene conversion) of the component a1 was 11100, and the viscosity (25° C.) of the component a1 was 1550 Pa·s.

[0129] <Preparation of Curable Resin Composition>

[0130] Example 1

[0131] 100 parts by mass of polyisobutylene (a1) having acryloxyethoxyphenyl group as the component (A) of the present invention, 7.8 parts by mass of bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide (Omnirad 819 manufactured by IGM Resins BV) as the component (B) (b1), and a defoamer (BYK-1799 manufactured by BYK-Chemie, dynamic viscosity (25° C.): 158 mm) containing no organic solvent and no methoxysilyl, ethoxysilyl or (meth)acryloyl silicone compound and a hydrophobic solid as the component (c1) were added. 2 / s) 0.9 parts by mass, isobornyl acrylate (IBX-A manufactured by Kyoeisha Chemical Co., Ltd.) as the (D) component (d1) 65 parts by mass, and lauryl acrylate (LA manufactured by Kyoeisha Chemical Co., Ltd.) as the (d2) 22 parts by mass were mixed at room temperature (25° C.) for 60 minutes using a planetary mixer under light shielding to obtain Example 1 as a curable resin composition containing no organic solvent.

[0132] Example 2

[0133] In Example 1, except having changed the (c1) component from 0.9 mass parts to 1.8 mass parts, it carried out similarly to Example 1, and obtained Example 2 which does not contain an organic solvent.

[0134] Example 3

[0135] In Example 1, except having changed the (c1) component from 0.9 mass parts to 3.6 mass parts, it carried out similarly to Example 1, and obtained Example 3 which does not contain an organic solvent.

[0136] Example 4

[0137] In Example 1, instead of component (c1), dimethylpolysiloxane (KF-96-100 cps manufactured by Shin-Etsu Chemical Co., Ltd., dynamic viscosity (25° C.): 100 mm / s) containing no organic solvent, having no methoxysilyl group, no ethoxysilyl group, and no (meth)acryloyl group, and having both ends blocked by trimethylsilyl groups was used as component (c2). 2 / s), except that the above-mentioned contents were 0.2% to 0.1% pyrrolidone, the mixture was prepared in the same manner as in Example 1 to obtain Example 4 containing no organic solvent.

[0138] Comparative Example 1

[0139] In Example 1, except for excluding (c1), the same method as in Example 1 was carried out to obtain Comparative Example 1 containing no organic solvent.

[0140] Comparative Example 2

[0141] Comparative Example 2 containing no organic solvent was prepared in the same manner as in Example 1 except that a defoaming agent containing no organic solvent and containing an organic polymer other than a silicone compound (BYK-1790 manufactured by BYK-Chemie) was used as component (c′1) instead of component (c1).

[0142] Comparative Example 3

[0143] In Example 1, a defoaming agent (BYK-066N manufactured by BYK-Chemie) containing diisobutyl ketone as an organic solvent and a silicone compound without methoxysilyl groups, ethoxysilyl groups and (meth)acryloyl groups was used as the (c'2) component instead of the (c1) component. The same preparation as in Example 1 was carried out to obtain Comparative Example 3 containing an organic solvent.

[0144] Comparative Example 4

[0145] In Example 1, except that a defoaming agent (BYK-067A manufactured by BYK-Chemie) containing propylene glycol as an organic solvent and a silicone compound without methoxysilyl groups, ethoxysilyl groups and (meth)acryloyl groups was used as component (c'3) instead of component (c1), the same method as in Example 1 was followed to obtain Comparative Example 4 containing an organic solvent.

[0146] Comparative Example 5

[0147] Comparative Example 5 containing no organic solvent was prepared in the same manner as in Example 1 except that a silicone oligomer containing no organic solvent and having an acryloyl group and a methoxy group in a side chain (KR-513 manufactured by Shin-Etsu Chemical Co., Ltd.) was used as component (c'4) instead of component (c1).

[0148] The test methods used in the examples and comparative examples in Table 1 are as follows. In addition, "-" in the table means that the measurement was not performed.

[0149] (1) Evaluation of repellency during screen printing

[0150] Using a SUS screen printing plate with a mesh size of 110 μm, each curable resin composition was applied to a polytetrafluoroethylene sheet by manual scraper printing at 25°C. Visually confirm whether each curable resin composition is rejected on the polytetrafluoroethylene sheet. The results are summarized in Table 1. Regarding the evaluation, the polytetrafluoroethylene sheet without rejection is "qualified", and the polytetrafluoroethylene sheet with obvious rejection is "unqualified". It should be noted that polytetrafluoroethylene has the same surface tension as the electrolyte membrane.

[0151] (2) Evaluation of defoaming properties during screen printing

[0152] Using a SUS screen printing plate with a mesh of 110 μm, each curable resin composition was applied to a polytetrafluoroethylene sheet by manual scraper printing at 25°C. Subsequently, the time for bubbles to disappear from the printed layer (thickness 50 μm) of the curable resin composition was visually confirmed as the defoaming time (seconds). It should be noted that the time measurement started immediately after printing and coating. The results are summarized in Table 1. From the perspective of line tact, the defoaming time is preferably within 60 seconds, more preferably within 50 seconds, and particularly preferably within 40 seconds.

[0153] (3) Determination of hardness

[0154] The thickness of each curable resin composition is set to 1mm, and ultraviolet rays with a cumulative light amount of 45kJ / m2 are irradiated to cure it, and a sheet-like cured product is prepared. The pressure surface of the A-type hardness meter (hardness meter) is maintained parallel to the test piece (a test piece in which 6 sheets of sheet-like cured products are overlapped and can be set to a state of thickness of 6mm), and pressed with a force of 10N at the same time, so that the pressure surface and the sample are closely fitted. The maximum value is read during the measurement, and the maximum value is used as the "hardness". The details are in accordance with JIS K 6253 (2012). It should be noted that the hardness is preferably 15 or more, more preferably 20 or more.

[0155] (4) Method for measuring elongation of cured product

[0156] The thickness of each curable resin composition was set to 1 mm, and the cumulative light intensity was 45 kJ / m 2 The ultraviolet rays were used to cure the film to produce a sheet-like cured product. A test piece was punched out with a No. 3 dumbbell and lines were marked at intervals of 20 mm on the test piece.

[0157] Fix it to the chuck in the same way as the tensile strength measurement, and stretch it at a tensile speed of 500 mm / min until the test piece is cut. During the measurement, the test piece is extended to widen the spacing between the markings, so the spacing between the markings is measured with a vernier caliper before the test piece is cut. The initial spacing between the markings is used as a reference and the extension ratio is set as "elongation (%)". Evaluation is performed based on the following references, and the results are shown in Table 2. It should be noted that the elongation is preferably 300% or more, and more preferably 410% or more from the viewpoint of high elongation.

[0158] (5) Tensile strength measurement

[0159] The thickness of the curable resin composition was set to 1 mm, and the cumulative light intensity was 45 kJ / m 2The test piece was made by punching out a test piece with a No. 3 dumbbell. The two ends of the test piece were fixed to the chuck in a straight line with the long axis of the test piece and the center of the chuck. The test piece was stretched at a tensile speed of 500 mm / min and the maximum load was measured. The strength at the maximum load was referred to as "tensile strength (MPa)". The details are in accordance with JIS K6251 (2010). It should be noted that the tensile strength is preferably 3.9 MPa or more, more preferably 4.2 MPa or more.

[0160] [Table 1]

[0161]

[0162] From Examples 1 to 4 in Table 1, it can be seen that the present invention is a curable resin composition capable of being applied by screen printing while maintaining high strength and high elongation properties of the cured product.

[0163] In addition, Comparative Example 1 of Table 1 is a curable resin composition that does not contain (c1) of the component (C) of the present invention. As a result, there is repulsion from the adherend during application based on screen printing, and the defoaming property is deteriorated. In addition, Comparative Example 2 is a curable resin composition that uses (c'1) instead of (c1) of the component (C) of the present invention. As a result, there is repulsion from the adherend during application based on screen printing, and the defoaming property is deteriorated. In addition, Comparative Examples 3 and 4 are curable resin compositions that use "(c'2) or (c'3) as a defoaming agent containing a solvent" instead of (c1) of the component (C) of the present invention. As a result, there is repulsion from the adherend during application based on screen printing, and the tensile strength of the cured product is deteriorated. In addition, Comparative Example 5 is a curable resin composition that uses (c'4) instead of (c1) of the component (C) of the present invention. There is repulsion from the adherend during application based on screen printing, and the tensile strength and elongation of the cured product are deteriorated.

[0164] Furthermore, (6) viscosity measurement and (7) water vapor permeability (water vapor barrier properties) were evaluated as follows.

[0165] (6) Viscosity measurement

[0166] The viscosity (Pa·s) of the curable resin composition was measured using a cone-plate viscometer (manufactured by Brook Field) under the following measurement conditions. Evaluation was performed based on the following criteria, and the results are shown in Table 2. The viscosity is preferably 100 Pa·s or less, more preferably 0.1 to 50 Pa·s, and particularly preferably in the range of 0.2 to 10 Pa·s.

[0167] From the results in Table 2, it can be seen that the viscosities of Examples 1 to 4 and Comparative Examples 1 and 3 to 5 are of the same level.

[0168] [Measurement conditions]

[0169] Cone type CPE-52, shear rate 10 (1 / s), temperature 25°C.

[0170] [Table 2]

[0171] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 (6) Viscosity (Pa·s) 5.3 5.5 5.2 5.5 5.4 - 4.9 6.4 5.3

[0172] (7) Moisture permeability (water vapor barrier)

[0173] The curable resin compositions of Examples 2 and 4 were poured into a frame of 200 mm×200 mm×1.0 mm. Then, the frame was irradiated with ultraviolet light at a cumulative light intensity of 45 kJ / m 2 The solidified product was irradiated with ultraviolet light for 20 seconds in a manner to obtain a sheet-like solidified product with a thickness of 1.0 mm. 5 g of calcium chloride (anhydrous) was placed in an aluminum cup with an opening of 30 mm in diameter and arranged in the cup in a manner to cover the solidified product. After measuring the "initial total weight" (g), the product was placed in a constant temperature thermostat at an ambient temperature of 40°C and a relative humidity of 95% for 24 hours, and the "total weight after placement" (g) was measured, and the moisture permeability (g / m 2 ·24h), and evaluated based on the following evaluation criteria. Examples 2 and 4 were both qualified. The detailed test method was in accordance with JIS Z 0208-1976. It should be noted that the moisture permeability is preferably less than 10 g / m 2 ·24h.

[0174] [Evaluation criteria]

[0175] Qualified: moisture permeability less than 10g / m 2 ·24h

[0176] Unqualified: moisture permeability is 10g / m 2 ·More than 24h.

[0177] This application is based on Japanese Patent Application No. 2020-146349 filed on August 31, 2020, the entire contents of which are incorporated herein by reference.

[0178] Possibility of Industrial Application

[0179] The present invention is made in view of the above situation, and is a curable resin composition that can be applied by screen printing while maintaining high strength and high elongation properties of the cured product, and can be used for various sealing purposes. In particular, it is effective as a curable sealant for fuel cells, so it is useful in industry.

[0180] Explanation of symbols

[0181] 1 Battery cell of polymer electrolyte fuel cell

[0182] 2 Diaphragm

[0183] 3a Air electrode (cathode)

[0184] 3b Fuel electrode (anode)

[0185] 4 Polymer Electrolyte Membrane

[0186] 5. Electrolyte membrane electrode assembly (MEA)

[0187] 6 Framework

[0188] 7 Adhesive or sealant

[0189] 8a Oxidizing gas flow path

[0190] 8b Fuel gas flow path

[0191] 9 Cooling water path

[0192] 10. Battery Pack

[0193] 11. Solid polymer fuel cell

Claims

1. A curable resin composition, characterized in that Containing the following components (A) to (C), (A) component: a polyisobutylene resin represented by the general formula (1); (B) component: free radical polymerization initiator; (C) component: a defoaming agent containing a silicone compound having no methoxysilyl group, no ethoxysilyl group and no (meth)acryloyl group and containing no organic solvent, [Chemistry 1] In formula (1), R 1 represents a monovalent or polyvalent aromatic hydrocarbon group, or a monovalent or polyvalent aliphatic hydrocarbon group which may have an aromatic ring, PIB represents a polyisobutylene skeleton containing -[CH2C(CH3)2]- units, R 4 represents a divalent hydrocarbon group having 2 to 6 carbon atoms which may contain an oxygen atom, R 2 and R 3 Each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms, and R 5 represents a hydrogen atom, a methyl group or an ethyl group, and n represents an arbitrary integer of 1 to 6.

2. The curable resin composition according to claim 1, wherein R of the component (A) 1 It is at least one selected from the group consisting of an aryl group having 6 to 18 carbon atoms, an arylene group having 6 to 18 carbon atoms, an arylalkyl group having 6 to 18 carbon atoms, or an alkylenearylenealkylene group having 6 to 18 carbon atoms.

3. The curable resin composition according to claim 1 or 2, characterized in that The component (C) is contained in an amount of 0.1 to 10 parts by mass based on 100 parts by mass of the component (A).

4. The curable resin composition according to claim 1 or 2, characterized in that The curable resin composition further contains a monofunctional monomer as the component (D), and the component (D) is a (meth)acrylate monomer having an alkyl group having 5 to 30 carbon atoms or a (meth)acrylate monomer having an alicyclic hydrocarbon group having 5 to 30 carbon atoms.

5. The curable resin composition according to claim 1 or 2, characterized in that Contains no organic solvents.

6. The curable resin composition according to claim 1 or 2, characterized in that The silicone compound of the component (C) is a compound having any structure of dimethylsiloxane, methylphenylsiloxane, or diphenylsiloxane.

7. The curable resin composition according to claim 4, wherein The component (C) is contained in an amount of 0.1 to 9 parts by mass based on 100 parts by mass of the total amount of the component (A) and the component (D).

8. The curable resin composition according to claim 1 or 2, wherein The component (B) is a photoradical polymerization initiator or an organic peroxide.

9. A curable sealant for a fuel cell, characterized in that , A curable resin composition comprising the curable resin composition according to claim 1 or 2.

10. The curable sealant for a fuel cell according to claim 9, wherein: The curable sealant for a fuel cell is used for any member selected from the group consisting of a separator, a frame, an electrolyte membrane, a fuel electrode, an air electrode, and an electrolyte membrane electrode assembly as a member in a fuel cell.

11. A cured product of the curable resin composition according to claim 1 or 2.

12. A fuel cell, characterized in that: Include: any seal selected from the group consisting of a seal between adjacent separators in a fuel cell and a seal between a frame of a fuel cell and an electrolyte membrane or an electrolyte membrane electrode assembly, The optional seal is the cured product according to claim 11.

13. A sealing method for sealing at least a portion between at least two flanges of a sealed component having at least two flanges, characterized in that: At least one of the flanges is permeable to active energy rays, and the method comprises: A step of applying the curable resin composition according to claim 1 or 2 to at least one surface of the flange, a step of bonding one flange coated with the curable resin composition and another flange via the curable resin composition; and The step of irradiating the flange that can transmit the active energy ray with active energy rays to cure the curable resin composition and seal at least a portion between the at least two flanges.

14. A sealing method for sealing at least a portion between at least two flanges of a sealed component having at least two flanges, characterized in that: include: a step of applying the curable resin composition according to claim 1 or 2 to at least one of the flanges, a step of irradiating the applied curable resin composition with active energy rays to cure the curable resin composition, thereby forming a gasket composed of a cured product of the curable resin composition; and The step of placing another flange on the gasket and press-bonding the one flange and the other flange coated with the curable resin composition with the gasket interposed therebetween to seal at least a portion between the at least two flanges.

15. A sealing method for sealing at least a portion between at least two flanges of a sealed component having at least two flanges, characterized in that: a step of disposing a gasket forming mold on at least one of the flanges; a step of injecting the curable resin composition according to claim 1 or 2 into at least a portion of a gap between the gasket forming mold and the one flange on which the mold is disposed, a step of irradiating the curable resin composition with the active energy ray to cure the curable resin composition, thereby forming a gasket composed of a cured product of the curable resin composition; the step of removing the mold from the one flange, and A step of arranging another flange on the gasket and press-bonding the one flange and the other flange with the gasket interposed therebetween, thereby sealing at least a portion between the at least two flanges.