A supported manganese / cerium low-temperature honeycomb denitrification catalyst and its preparation method

By loading CeO2 and MnOx on the honeycomb carrier, a supported manganese/cerium low-temperature honeycomb denitrification catalyst suitable for low temperature conditions was prepared, which solved the problem of NOx emissions in cement kiln flue gas being difficult to meet stringent standards and achieved efficient and economical denitrification. Low temperature denitrification effect.

CN115888693BActive Publication Date: 2024-10-15ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211312192.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2024-10-15
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

Existing cement kiln flue gas denitrification technology is difficult to meet the increasingly stringent ultra-low NOx emission standards, especially under low-temperature flue gas conditions, and commercial catalysts cannot be effectively applied.

Method used

The vacuum impregnation process is used to load cerium dioxide (CeO2) and manganese oxide (MnOx) on the integral honeycomb carrier to prepare a supported manganese/cerium low-temperature honeycomb denitration catalyst, which is suitable for low-temperature conditions of 100-300°C.

Benefits of technology

It achieves efficient NOx denitration in the range of 100-300°C, reduces production costs, and shows excellent low-temperature denitration performance and stability in actual cement kiln flue gas pipelines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115888693B_ABST
    Figure CN115888693B_ABST
Patent Text Reader

Abstract

The invention discloses a supported manganese / cerium low-temperature honeycomb denitration catalyst and a preparation method thereof, and relates to the fields of catalyst preparation and environmental protection. The supported manganese / cerium low-temperature honeycomb denitration catalyst is composed of cerium dioxide (CeO2) and manganese oxide (MnO x ) as the main active ingredient, and a formed honeycomb carrier as the matrix material. The loaded manganese / cerium low-temperature honeycomb denitration catalyst is prepared by impregnating the formed honeycomb carrier in a metal salt solution, and cyclically impregnating and calcining under high vacuum conditions, and finally preparing the desired catalyst. The loaded manganese / cerium low-temperature honeycomb denitration catalyst of the present invention has been subjected to pilot performance evaluation in an actual cement kiln flue gas duct, showing excellent low-temperature denitration performance and stability. The loaded manganese / cerium low-temperature honeycomb denitration catalyst of the present invention not only has a simple preparation method, but the materials used for the active components are all environmentally friendly materials with little pollution to the environment, and also fills the gap in the industrial application of the domestic loaded manganese / cerium low-temperature honeycomb denitration catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental protection technology and low-temperature denitration, and specifically relates to a supported manganese / cerium low-temperature honeycomb denitration catalyst and a preparation method thereof. Background Art

[0002] my country is a country with a large infrastructure industry. Taking the cement industry as an example, the building materials industry has made great contributions to my country's economic and social development. At the same time, large-scale cement production has also brought about environmental pollution problems that cannot be ignored. According to statistics, my country's cement industry emits nitrogen oxides (NO x ) accounts for about 10-12% of the total industrial emissions in China, second only to thermal power generation and automobile exhaust. As environmental protection policies become increasingly stringent, more and more local governments have formulated emission standards that are more stringent than national standards. x Emission standards increased to 100mg / m 3 , the ultra-low emission standard is 50mg / m 3 At present, the widely used cement denitrification technology (selective non-catalytic reduction, SNCR) is difficult to meet the increasingly stringent emission standards. For the cement industry, in order to achieve ultra-low emission requirements, SNCR technology can be combined with selective catalytic reduction (SCR) technology to meet NO x Ultra-low emission standards requirements.

[0003] Among the combined technologies, SCR flue gas denitrification technology is currently recognized in China and has achieved good practical application. Among them, SCR technology with NH3 as a reducing agent (NH3-SCR) is a common flue gas treatment technology for fixed sources (such as power plants and waste incineration plants). The flue gas in the cement kiln passes through the SNCR technology. At the same time, the actual operating conditions fluctuate greatly, the exhaust conditions are unstable, and the flue gas waste heat is reused, the site is limited and other factors make the exhaust flue gas temperature usually low, fluctuating between 120-300℃. At present, the operating temperature of the commercial V2O5-WO3 / TiO2 catalyst is 300-450℃, which cannot be applied to the actual low-temperature flue gas denitrification.

[0004] Therefore, according to the actual characteristics of cement kiln flue gas, the development and design of catalysts with low-temperature denitrification performance is of great significance to the further control of cement kiln flue gas in my country. Low-temperature denitrification catalysts not only have better environmental applicability, but also can reduce energy consumption and save costs. Therefore, the development of a new type of low-temperature denitrification catalyst not only fully meets the current market demand of the low-temperature flue gas denitrification industry, but also fills the gap in domestic low-temperature denitrification catalysts. Summary of the invention

[0005] The purpose of the present invention is to provide a supported manganese / cerium low-temperature honeycomb denitration catalyst and its preparation process. x / CeO2) as the main active ingredient of denitrification catalysts, however, these catalysts are only powder catalysts in the laboratory stage and cannot be actually used in flue gas ducts. x The preparation process and conditions of CeO2 denitrification catalyst affect the denitrification performance of the monolithic catalyst.

[0006] Therefore, the present invention innovatively loads CeO2 on the monolithic honeycomb carrier by vacuum impregnation process, and then the active component MnO x A supported manganese / cerium low-temperature honeycomb denitrification catalyst was obtained by loading it on CeO2, and its low-temperature denitrification performance was tested in an actual cement kiln flue gas duct.

[0007] The present invention is implemented by the following technical solutions:

[0008] A method for preparing a supported manganese / cerium low-temperature honeycomb denitration catalyst, the method for preparing the supported manganese / cerium low-temperature honeycomb denitration catalyst comprising the following process steps:

[0009] (1) First, a cerium salt solution with a concentration of 20-100 g / L is prepared and poured into a specific vacuum reactor;

[0010] (2) placing the honeycomb carrier in the vacuum reactor of step (1), wherein the pressure in the vacuum reactor is -0.1 MPa to 1 MPa, and immersing the carrier for a period of time under vacuum conditions;

[0011] (3) After the impregnation is completed, the honeycomb catalyst is taken out and the water in the honeycomb catalyst is drained. The drying time is 12h-24h;

[0012] (4) After the water is dried, the honeycomb catalyst is placed in a calcining furnace for calcining;

[0013] (5) repeating the impregnation and calcination processes of steps (2) to (4) several times;

[0014] (6) preparing a manganese salt solution with a concentration of 5-20 g / L and pouring it into another vacuum reactor;

[0015] (7) placing the calcined honeycomb substrate in a vacuum reactor filled with a manganese salt solution, wherein the pressure in the vacuum reactor is -0.1 MPa to 1 MPa, and immersing the substrate in the vacuum condition for a period of time;

[0016] (8) After the impregnation is completed, the honeycomb catalyst is taken out and the water in the honeycomb catalyst is dried for 12h-24h.

[0017] (9) After the water is dried, the honeycomb catalyst is placed in a calcining furnace for calcining;

[0018] (10) Repeat the impregnation process and calcination process of steps (7) to (9) several times to obtain the supported manganese / cerium low-temperature honeycomb denitrification catalyst.

[0019] The supported manganese / cerium low-temperature honeycomb denitration catalyst and the preparation method thereof of the present invention also include the following preferred embodiments.

[0020] In a preferred embodiment of the present invention, the cerium salt added in step (1) is at least one of cerium nitrate, cerium chloride or cerium carbonate.

[0021] In a preferred embodiment of the present invention, the vacuum impregnation time in step (2) is 30 min-60 min.

[0022] In a preferred embodiment of the present invention, the calcination temperature in step (4) is 300°C-600°C, the heating rate is 5°C / min-20°C / min, and the calcination time is 2h-6h.

[0023] In a preferred embodiment of the present invention, the manganese salt in step (5) is at least one of manganese acetate, manganese chloride or manganese sulfate.

[0024] In a preferred embodiment of the present invention, the vacuum impregnation time in step (6) is 30 min-60 min.

[0025] In a preferred embodiment of the present invention, the calcination temperature in step (6) is 300°C-600°C, the heating rate is 5°C / min-20°C / min, and the calcination time is 2h-6h.

[0026] In a preferred embodiment of the present invention, the vacuum impregnation process and the calcination process in step (8) are cycled 1-5 times.

[0027] In the preferred embodiment of the present invention, the formed integral honeycomb as a honeycomb carrier can be a V2O5-WO3 / TiO2 medium-temperature denitration catalyst, cordierite honeycomb ceramic, mullite, or alumina ceramic on the market, preferably a V2O5-WO3 / TiO2 medium-temperature denitration catalyst. Commercial V2O5-WO3 / TiO2 medium-temperature denitration catalysts usually need to be made into a monolithic type because, in actual use, the catalyst needs to be subjected to the scouring of high-speed dust, resulting in the loss of the catalyst. The biggest feature of the monolithic type is that the component structure is uniform, and the original activity can still be maintained after scouring. However, because it is a monolithic type, the relative cost is relatively high. In actual application, the low-temperature SCR denitration catalyst is generally installed after the dust removal facility, and will not be scour by high-speed dust to cause the catalyst to wear. Therefore, there is no need to make a monolithic catalyst. The present invention uses V2O5-WO3 / TiO2 catalyst as a carrier to prepare a manganese / cerium low-temperature honeycomb denitration catalyst, which can avoid the influence of the molding process on the catalyst performance and can also greatly reduce the cost, which is one of the best solutions.

[0028] A supported manganese / cerium low-temperature honeycomb denitration catalyst is prepared by the above method and can be used as a catalyst for removing nitrogen oxides in cement kilns under low-temperature conditions.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention uses commercially available honeycomb catalyst as a carrier, and adds active components of cerium dioxide (CeO2) and manganese oxide (MnO x ), and adopts the vacuum impregnation production process to prepare a supported low-temperature honeycomb denitrification catalyst suitable for 100-300℃. It is mainly achieved through the following aspects:

[0031] (1) Vacuum impregnation is relatively simple in process compared to other methods for loading active components of catalysts, and can reduce the production cost of the integral honeycomb catalyst. In addition, the integral honeycomb catalyst has already gone through the high-temperature calcination stage, and the catalyst is already in a dense sintered state. The present invention places the integral catalyst carrier into a salt solution containing active components, and uses the vacuum impregnation method to fully load the active components on the catalyst carrier.

[0032] (2) CeO2 has high efficiency in oxygen storage and release and unique redox properties. After CeO2 loading is completed, the same method is used to load MnO x Loaded on CeO2, a supported honeycomb catalyst with excellent denitrification activity was obtained.

[0033] (3) When the monolithic honeycomb V2O5-WO3 / TiO2 medium-temperature denitration catalyst is used as a carrier, the present invention has another advantage that CeO2 is first loaded, so that V2O5 and CeO2 can interact with each other to enhance the low-temperature activity of the catalyst itself (Journal of Molecular Catalysis. A, Chemical, 356 (2012) 121-127), and at the same time, a step-by-step loading method is adopted to effectively block the interaction between V2O5 and MnO x The mutual inhibition between them (Catalysis Letters, 141 (2011) 1237-1242) ensures its low-temperature activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the element distribution diagram of the supported manganese / cerium low-temperature honeycomb deNOx catalyst prepared in Example 3.

[0035] Figure 2 This is a graph showing the denitration performance data of the supported manganese / cerium low-temperature honeycomb denitration catalyst prepared in Examples 1-3.

[0036] Figure 3 A physical picture of the supported manganese / cerium low-temperature honeycomb denitrification catalyst prepared in Example 4.

[0037] Figure 4 Denitration performance data of the supported manganese / cerium low-temperature honeycomb denitration catalyst prepared in Example 4.

[0038] Figure 5 Stability data graph of the supported manganese / cerium low-temperature honeycomb deNOx catalyst prepared in Example 4. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0040] Example 1

[0041] A method for preparing a cerium low-temperature honeycomb denitration catalyst comprises the following implementation steps: (1) first preparing a cerium nitrate solution with a concentration of 20 g / L and pouring it into a specific vacuum reactor; (2) placing a honeycomb carrier in a vacuum reactor for vacuum impregnation, wherein the pressure in the vacuum reactor is -0.1 MPa, and the vacuum impregnation time is 30 min; (3) after the impregnation is completed, taking out the honeycomb catalyst, and draining the water in the honeycomb carrier for 12 h; (4) after the water is drained, placing the honeycomb carrier in a calcining furnace for calcination, wherein the calcination temperature is 400°C, the heating rate is 5°C / min, and the calcination time is 2 h; (5) the above process is repeated 3 times to obtain the cerium low-temperature honeycomb denitration catalyst.

[0042] Example 2

[0043] A method for preparing a supported manganese / cerium low-temperature honeycomb denitration catalyst comprises the following steps: (1) first preparing a cerium nitrate solution with a concentration of 20 g / L and pouring it into a specific vacuum reactor; (2) placing a honeycomb carrier in a vacuum reactor for vacuum impregnation, wherein the pressure in the vacuum reactor is -0.1 MPa, and the vacuum impregnation time is 30 min; (3) after the impregnation is completed, the honeycomb carrier is taken out, and the water in the honeycomb carrier is drained for 12 h; (4) after the water is drained, the honeycomb carrier is placed in a calcining furnace for calcination, wherein the calcination temperature is 400°C, the heating rate is 5°C / min, and the calcination time is 2 h; (5) the above process is repeated for 1 h. The process is repeated for 3 times; (6) a manganese acetate solution with a concentration of 10 g / L is prepared and poured into a vacuum reactor; (7) the calcined honeycomb carrier is placed in a vacuum reactor filled with manganese acetate solution, the pressure in the vacuum reactor is -0.1 MPa, and the vacuum impregnation time is 30 min; (8) after the impregnation is completed, the honeycomb carrier is taken out, and the water in the honeycomb carrier is drained for 12 h; (9) after the water is drained, the honeycomb carrier is placed in a calcination furnace for calcination at a temperature of 350 °C, a heating rate of 5 °C / min, and a calcination time of 2 h, thereby obtaining the supported manganese / cerium low-temperature honeycomb deNOx catalyst.

[0044] Example 3

[0045] A method for preparing a supported manganese / cerium low-temperature honeycomb denitration catalyst comprises the following steps: (1) first preparing a cerium nitrate solution with a concentration of 20 g / L and pouring it into a specific vacuum reactor; (2) placing a honeycomb carrier in a vacuum reactor for vacuum impregnation, wherein the pressure in the vacuum reactor is -0.1 MPa, and the vacuum impregnation time is 30 min; (3) after the impregnation is completed, taking out the honeycomb catalyst, and draining the water in the honeycomb carrier for 12 h; (4) after the water is drained, placing the honeycomb carrier in a calcining furnace for calcination, wherein the calcination temperature is 400°C, the heating rate is 5°C / min, and the calcination time is 2 h; (5) the above process is repeated for 3 cycles. times; (6) preparing a manganese acetate solution with a concentration of 10 g / L and pouring it into a vacuum reactor; (7) placing the calcined honeycomb carrier in a vacuum reactor filled with manganese acetate solution, the pressure in the vacuum reactor is -0.1 MPa, and the vacuum impregnation time is 30 min; (8) after the impregnation is completed, taking out the honeycomb carrier and draining the water in the honeycomb carrier for 12 h; (9) after the water is drained, placing the honeycomb carrier in a calcination furnace for calcination at a temperature of 350 ° C, a heating rate of 5 ° C / min, and a calcination time of 2 h; (10) repeating the above process twice to obtain the supported manganese / cerium low-temperature honeycomb deNOx catalyst.

[0046] Figure 1 This is the element distribution diagram of the supported manganese / cerium low-temperature honeycomb denitration catalyst prepared in Example 3 of the present invention. Figure 1 It can be seen that Mn and Ce are evenly distributed on the catalyst carrier. According to the ratio of reactants added in Example 3, the content of Mn is relatively low, so the signal detected in the figure is relatively low.

[0047] The catalysts prepared in Example 1, Example 2 and Example 3 were subjected to a laboratory stage modular low-temperature denitration performance test, specifically comprising the following steps: (1) a modular catalyst of 5 cm in length, 4 cm in width and 4 cm in height was cut and placed in a fixed tubular furnace reaction tube; (2) the reactor inlet contained 500 ppm NO, 500 ppm NH3, 5% O2, and the remainder was N2, the total gas flow rate was 2.1 L / min, and the test reaction temperature was 100°C-300°C. The denitration performance of the catalysts prepared in Examples 1-3 is shown in FIG. Figure 2 As shown. Figure 2 It can be seen that the supported manganese / cerium low-temperature honeycomb denitration catalyst prepared in the present invention can achieve a denitration efficiency of 30%-70% in flue gas at 100°C-300°C. And at the same temperature, the denitration performance of the cerium low-temperature honeycomb denitration catalyst obtained by only loading cerium in Example 1 is significantly lower than that of the supported manganese / cerium low-temperature honeycomb denitration catalyst of the present invention.

[0048] Example 4

[0049] A supported manganese / cerium low-temperature honeycomb denitration catalyst and a preparation method thereof, comprising the following implementation steps: (1) first preparing a cerium nitrate solution with a concentration of 20 g / L and pouring it into a specific vacuum reactor; (2) placing a honeycomb carrier in a vacuum reactor for vacuum impregnation, the pressure in the vacuum reactor is -0.1 MPa, and the vacuum impregnation time is 60 min; (3) after the impregnation is completed, the honeycomb carrier is taken out, and the water in the honeycomb carrier is drained for 12 hours; (4) after the water is drained, the honeycomb carrier is placed in a roasting furnace for roasting treatment, the roasting temperature is 350°C, the heating rate is 5°C / min, and the roasting time is 2 hours; (5) the above process is repeated for 3 times ; (6) Prepare a manganese acetate solution with a concentration of 10g / L and pour it into another vacuum reactor; (7) Place the calcined honeycomb carrier in a vacuum reactor filled with a manganese salt solution, the pressure in the vacuum reactor is -0.1MPa, and the vacuum impregnation time is 60nin; (8) After the impregnation is completed, take out the honeycomb carrier and drain the water in the honeycomb carrier for 12h; (9) After the water is drained, place the honeycomb carrier in a calcination furnace for calcination at a temperature of 300℃, a heating rate of 5℃ / min, and a calcination time of 2h; (10) Repeat the above process twice to obtain the supported manganese / cerium low-temperature honeycomb deNOx catalyst.

[0050] The catalyst prepared in Example 4 was subjected to an actual industrial denitration performance test, which specifically included the following steps: (1) According to the experimental steps and processes of Example 4, 2m 3 The loaded manganese / cerium low-temperature honeycomb denitrification catalyst (length 100 cm, width 15 cm, height 15 cm, the actual catalyst is shown in the figure), and the catalyst is installed in the flue gas duct; (2) the actual NO x The concentration is about 100 mg / m 3 -300mg / m 3 , the flue gas velocity is 4m / s, the ammonia injection rate is 1.5L / h, the O2 reference value is 10%; the monitoring reaction temperature is 120℃-300℃. Figure 4 It can be seen that the supported manganese / cerium low-temperature honeycomb denitrification catalyst prepared in the present invention exhibits excellent low-temperature denitrification performance in the actual cement kiln flue gas pipeline, and the denitrification efficiency in the flue gas at 120°C-300°C can reach 60%-95%. At the same time, the stability of the catalyst (such as Figure 5 As shown in Figure 2, the catalyst can maintain a denitration efficiency of 70%-75% in flue gas at 175°C. The supported manganese / cerium low-temperature honeycomb denitration catalyst prepared by the present invention successfully converts MnO into xThe / CeO2 active component is loaded on the honeycomb carrier, which fully realizes the synergistic effect between cerium and manganese and realizes the industrial application of loaded manganese / cerium low-temperature honeycomb denitrification catalyst.

[0051] The supported manganese / cerium low-temperature honeycomb denitration catalyst of the present invention has been tested for performance in an actual cement kiln flue gas pipeline, showing excellent low-temperature denitration performance and stability. The supported manganese / cerium low-temperature honeycomb denitration catalyst of the present invention not only has a simple preparation method, but also uses environmentally friendly materials for the active components, which has little pollution to the environment. It also fills the gap in the industrial application of supported manganese / cerium low-temperature honeycomb denitration catalysts in China.

[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a supported manganese / cerium low-temperature honeycomb denitrification catalyst, characterized in that: The following steps are involved: (1) First, a cerium salt solution with a concentration of 10-100 g / L is prepared and poured into a vacuum reactor; (2) placing the honeycomb carrier in a vacuum reactor filled with a cerium salt solution for impregnation, wherein the pressure in the vacuum reactor is -0.1 MPa to 1 MPa during the impregnation process; (3) After the impregnation is completed, the honeycomb carrier is taken out and the water in the honeycomb carrier is drained; (4) placing the honeycomb carrier into a calcining furnace for calcining; (5) repeating the impregnation and calcination processes of steps (2) to (4) several times; (6) preparing a manganese salt solution with a concentration of 5-50 g / L and pouring it into another vacuum reactor; (7) placing the calcined honeycomb substrate in a vacuum reactor filled with a manganese salt solution for impregnation, wherein the pressure in the vacuum reactor is -0.1 MPa to 1 MPa during the impregnation process; (8) After the impregnation is completed, the honeycomb carrier is taken out and the water in the honeycomb catalyst carrier is drained; (9) placing the honeycomb carrier into a calcining furnace for calcining; (10) Repeat the impregnation process and calcination process of steps (7) to (9) several times to obtain the supported manganese / cerium low-temperature honeycomb denitrification catalyst; The immersion time in step (2) is 30 min to 60 min; The calcination temperature in step (4) is 300°C-600°C, the heating rate is 5°C / min-20°C / min, and the calcination time is 2h-6h; The immersion time in step (7) is 30 min to 60 min; The calcination temperature in step (9) is 300°C-600°C, the heating rate is 5°C / min-20°C / min, and the calcination time is 2h-6h; The honeycomb carrier is a V2O5-WO3 / TiO2 medium-temperature denitration catalyst.

2. The method for preparing a supported manganese / cerium low-temperature honeycomb denitration catalyst according to claim 1, characterized in that: The cerium salt described in step (1) is at least one of cerium nitrate, cerium chloride or cerium carbonate.

3. The method for preparing a supported manganese / cerium low-temperature honeycomb denitration catalyst according to claim 1, characterized in that: The manganese salt in step (6) is at least one of manganese acetate, manganese chloride or manganese sulfate.

4. The method for preparing a supported manganese / cerium low-temperature honeycomb denitration catalyst according to claim 1, characterized in that: The impregnation process and the calcination process described in steps (5) and (10) are cycled 1 to 5 times.

5. A supported manganese / cerium low-temperature honeycomb denitrification catalyst, characterized in that: The method is prepared by the method according to any one of claims 1 to 4.