A composite current collector heat-resistant base film and preparation method thereof

By using PP and PET composite materials in the composite current collector base film and adding modified carbon nanotubes and silica to form a filler network, the problem of insufficient heat resistance and strength of the base film is solved, and a higher Heat resistance and strength, suitable for improving battery safety and energy density.

CN118027559BActive Publication Date: 2024-10-15扬州博恒新能源材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410178577.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-09
Publication Date
2024-10-15
Estimated Expiration
2044-02-09

AI Technical Summary

Technical Problem

Existing composite current collector base films have problems with poor heat resistance and poor strength. In particular, PP and PET base films do not perform well at high temperatures and have high costs.

Method used

A composite of PP and PET is used as the base film material, and carbon nanotubes, silica and cellulose are added as fillers. Its compatibility and bonding strength are improved through modification treatment to form a filler network to enhance the heat resistance of the base film. sex and intensity.

Benefits of technology

Significantly improves the heat resistance and strength of the base film, reduces the problem of uneven strength caused by the migration of small molecules of the compatibilizer, enhances the tensile properties of the base film and the bonding effect of the metal layer, and improves the safety and energy density of the battery .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004702760400000121
    Figure BDA0004702760400000121
Patent Text Reader

Abstract

The present application relates to the technical field of current collectors, and specifically discloses a composite current collector heat-resistant base film, a preparation method and an application. The composite current collector heat-resistant base film comprises the following substances in parts by weight: 1‑99 parts of PP; 1‑99 parts of PET; 0.1‑10 parts of filler, wherein the filler comprises one or more of carbon nanotubes, silica or cellulose. The preparation method thereof is as follows: S1, raw material blending; S2, melt extrusion; S3, stretching. The composite current collector heat-resistant base film of the present application can be used for the current collector, which has the advantages of heat resistance, tensile strength, high toughness, high strength, etc.; in addition, the preparation method of the present application has the advantages of simple process and easy operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite current collectors, and more specifically, to a composite current collector heat-resistant base film, a preparation method and an application thereof. Background Art

[0002] Composite current collector is a new material that deposits a metal layer (a sandwich structure of metal layer + organic film + metal layer with a thickness of about 1μm) on the surface of an ultra-thin organic polymer film. It can replace the traditional electrolytic copper foil of the negative electrode current collector or the rolled aluminum foil of the positive electrode current collector. The outstanding advantage of the composite current collector is that the amount of metal material used is reduced, and the amount used is only about 1 / 3 to 1 / 5 of the original, which effectively reduces the material cost; secondly, due to the use of thin films in the composite current collector, the weight of the battery is reduced, the thinning is reduced, and the active material is increased, thereby effectively increasing the energy density of the battery by 5%-10%, and the cycle life of the battery is increased by 5%; the application of composite current collector materials can greatly reduce the probability of combustion caused by battery short circuit, which can effectively solve the problem of battery safety.

[0003] At present, the base films used in composite current collectors are mostly made of PP (polypropylene), PET (polyethylene terephthalate), and PI (polyimide), but PP has the defect of poor heat resistance, PET has the defect of poor chemical stability, and PI has the defect of high cost. That is, the current base films still have the defects of poor heat resistance and poor strength. Summary of the invention

[0004] In order to improve the defects of poor heat resistance and poor strength of the base film, the present application provides a composite current collector heat-resistant base film, a preparation method and application, using the following technical solutions:

[0005] In a first aspect, the present application provides a composite current collector heat-resistant base film, comprising the following substances in parts by weight:

[0006] PP 1-99 copies;

[0007] PET 1-99 parts;

[0008] The filler is 0.1-10 parts, and the filler includes one or more of carbon nanotubes, silicon dioxide or cellulose.

[0009] By adopting the above technical solution, PP and PET are used as the main materials of the base film, which can give the base film excellent heat resistance and strength, and improve the defects of the base film prepared by a single material. Adding carbon nanotubes in the base film, carbon nanotubes have an excellent aspect ratio, which can not only serve as reinforcing particles to improve the strength of the base film; but also reduce the Tg difference between PP and PET and improve the compatibility between PP and PET. Carbon nanotubes can pull at the interface between PP and PET, reduce the sea island structure formed in PP and PET, play a role in increasing volume, and improve the interface bonding effect between PP and PET, thereby improving the tensile effect and strength of the base film. The compatibility of PP and PET can be improved without adding a compatibilizer to the base film, which reduces the possibility of uneven strength of the base film caused by the migration of small molecules of the compatibilizer, so that the base film obtains uniform strength.

[0010] As a filler, silica can effectively fill the base film and introduce anchoring sites in the base film, thereby improving the bonding effect between PP and PET. The addition of cellulose can use the fiber structure to pull the components in the base film, thereby improving the bonding strength between PP and PET.

[0011] By combining carbon nanotubes, silica and cellulose, a filler network can be formed in the base film, which not only improves the compatibility of PP and PET, but also further improves the bonding strength of the base film and stably improves the strength of the base film.

[0012] Optionally, the filler is a filler modified by a modifier, and the modifier includes one or more of rare earth compounds, maleic anhydride, silk fibroin, and a silane coupling agent.

[0013] By adopting the above technical solution, the filler is modified with a rare earth compound, and the rare earth compound can form a coating structure on the surface of the filler, which can effectively reduce the surface energy of the filler surface and improve the dispersion uniformity of the filler in the base film. At the same time, since the rare earth particles can interact with the macromolecular chains in the base film, the bonding effect between the filler and the base film can be improved.

[0014] Maleic anhydride is used to modify the filler. Maleic anhydride can act as a coupling agent to improve the dispersion and bonding effect of the filler. At the same time, the addition of maleic anhydride can introduce anhydride groups on PP, increase the viscosity of PP, improve the compatibility and bonding strength between the components in the base film, and stably improve the strength of the base film.

[0015] The filler is modified by silk fibroin. The aromatic amino acid residues in silk fibroin can form a strong π-π interaction on the filler surface, thereby improving the uniformity of the filler dispersion in the base film and making the base film obtain a uniform reinforcement effect. At the same time, silk fibroin can also improve the compatibility of PP and PET, further improving the strength of the base film.

[0016] The filler is modified by using a silane coupling agent, which can improve the dispersion effect of the filler and make the filler uniformly enhance the strength of the base film.

[0017] Optionally, the carbon nanotubes include carbon nanotubes modified with rare earth compounds, and the preparation of the rare earth-modified carbon nanotubes includes: configuring the carbon nanotubes into a dispersion, adding rare earth compounds to the dispersion, adjusting the pH to obtain a suspension, adding a flocculant to the suspension, sedimentation, centrifugation, retaining solids, and drying to obtain rare earth-modified carbon nanotubes.

[0018] By adopting the above technical scheme, the rare earth compound and the carbon nanotubes form ionic bonds through electrostatic attraction, and then the flocculant is used to stabilize the carbon nanotube surface to form a coating structure, that is, a core-shell structure, which can reduce the agglomeration of the carbon nanotubes and make the carbon nanotubes evenly dispersed in the base film; at the same time, it can also improve the compatibility of the carbon nanotubes and PP, stabilize and toughen the base film, and improve the strength of the base film.

[0019] Optionally, the rare earth ion concentration of the rare earth compound is 4-6%, and the pH is 8-9.

[0020] By adopting the above technical solution, the ion concentration of the rare earth compound is optimized. The appropriate concentration can enable the rare earth compound to form a uniform coating structure on the surface of the carbon nanotube, so that the carbon nanotube is evenly dispersed in the base film. If the concentration of the rare earth compound is too low, the rare earth compound is difficult to coat the surface of the carbon nanotube, and it is difficult to form a coating structure. If the concentration of the rare earth compound is too high, the rare earth compound is more likely to cause the hydrolysis reaction rate to be too fast, and it is difficult to control the adsorption effect of the rare earth compound on the surface of the carbon nanotube, and it is difficult to form a coating structure. The pH of the modification is optimized. At an appropriate pH, the rare earth compound can form a uniform and dense coating on the surface of the carbon nanotube, and stably reduce the agglomeration between the carbon nanotube particles.

[0021] Optionally, the carbon nanotubes also include carbon nanotubes modified with silk fibroin, and the preparation of the protein-modified carbon nanotubes includes: dispersing the carbon nanotubes in a phosphoric acid solution, ultrasonically mixing to obtain a suspension, adding degummed silk fibroin fibers to the suspension, homogenizing, centrifuging, retaining solids, and drying to obtain silk fibroin-modified carbon nanotubes.

[0022] By adopting the above technical solution, silk fibroin can form a strong π-π interaction with the surface of carbon nanotubes, so that the carbon nanotubes are evenly dispersed in the base film. Phosphoric acid is used as the dispersion liquid. First, due to the strong polarity of phosphoric acid, the carbon nanotubes can be fully dispersed in phosphoric acid; secondly, the silk fibroin fiber can be quickly dissolved and decomposed in phosphoric acid, so that the silk fibroin can be fully loaded on the carbon nanotubes. At the same time, due to the large number of polar groups in the silk fibroin, it can have a better binding effect with copper ions, that is, improve the binding between the base film and the metal layer.

[0023] Optionally, the silicon dioxide is silicon dioxide modified by a silane coupling agent, and the silane coupling agent includes KH-550 and KH-560.

[0024] Optionally, the silane coupling agent is prepared by adding equal masses of KH-550 and KH-560 into a container, heating for reaction, and cooling to obtain the silane coupling agent.

[0025] By adopting the above technical scheme, KH-550 and KH-560 are used to prepare silane coupling agents. KH-550 and KH-560 can form a network structure. The network structure is loaded with multiple alkoxy groups, which can combine with the active hydroxyl groups on the surface of silica to achieve grafting modification of silica, so that the silica particles form a structure that is connected but not in direct contact, thereby prompting silica to form a spatial network structure in the base film, further improving the strength and toughness of the base film.

[0026] In a second aspect, the present application provides a method for preparing a composite current collector heat-resistant base film, using the following technical solution:

[0027] A method for preparing a composite current collector heat-resistant base film comprises the following steps:

[0028] S1. Raw material blending: PP, PET and filler are mixed and heated to melt to obtain PP / PET mixed resin melt;

[0029] S2, melt extrusion: PP / PET intermixed resin melt is granulated and extruded to obtain mixed masterbatch, which is heated and melted again, and reaches the die head to form a thick sheet after passing through a metering pump, a filter, and an adapter;

[0030] S3. Stretching: After the thick sheet is stretched longitudinally, it is stretched transversely to obtain a heat-resistant base film.

[0031] Optionally, the heat-resistant base film is subjected to corona treatment.

[0032] By adopting the above technical solution and performing corona treatment on the heat-resistant base film, a rough structure can be formed on the surface of the heat-resistant base film, thereby improving the bonding strength between the heat-resistant base film and the metal layer.

[0033] In a third aspect, the present application provides an application of a composite current collector heat-resistant base film, using the following technical solution:

[0034] An application of a composite current collector heat-resistant base film, the above-mentioned composite current collector heat-resistant base film is applied to a composite current collector.

[0035] In summary, this application has the following beneficial effects:

[0036] 1. Since the present application adopts a composite of PP and PET as the main material of the base film, the base film can be endowed with excellent heat resistance and strength, and the defects of the base film prepared by a single material can be improved. Adding carbon nanotubes in the base film, carbon nanotubes have an excellent aspect ratio, which can not only serve as reinforcing particles to improve the strength of the base film; it can also reduce the Tg difference between PP and PET and improve the compatibility of PP and PET. Carbon nanotubes can be pulled at the interface between PP and PET, reduce the sea island structure formed in PP and PET, play a role of increasing volume, and improve the interfacial bonding effect of PP and PET, thereby improving the tensile effect and strength of the base film. The compatibility of PP and PET can be improved without adding a compatibilizer to the base film, which reduces the possibility of uneven strength of the base film caused by the migration of small molecules of the compatibilizer, so that the base film obtains uniform strength.

[0037] 2. In the present application, the rare earth compound and the carbon nanotubes form ionic bonds through electrostatic attraction, and then are stabilized on the surface of the carbon nanotubes by a flocculant to form a coating structure, that is, a core-shell structure, which can reduce the agglomeration of the carbon nanotubes and make the carbon nanotubes evenly dispersed in the base film; at the same time, it can also improve the compatibility of the carbon nanotubes and PP, stabilize and toughen the base film, and improve the strength of the base film.

[0038] 3. In the present application, the silk fibroin can form a strong π-π interaction with the surface of the carbon nanotubes, so that the carbon nanotubes are evenly dispersed in the base film. Phosphoric acid is used as the dispersion liquid. First, due to the strong polarity of phosphoric acid, the carbon nanotubes can be fully dispersed in phosphoric acid; secondly, the silk fibroin fibers can be quickly dissolved and decomposed in phosphoric acid, so that the silk fibroin can be fully loaded on the carbon nanotubes. At the same time, due to the large number of polar groups in the silk fibroin, it can have a better binding effect with copper ions, that is, improve the binding between the base film and the metal layer.

[0039] 4. In the present application, KH-550 and KH-560 are used to prepare silane coupling agents. KH-550 and KH-560 can form a network structure. The network structure is loaded with multiple alkoxy groups, which can combine with the active hydroxyl groups on the surface of silica to achieve grafting modification of silica, thereby forming a structure in which the silica particles are connected but not in direct contact, thereby prompting silica to form a spatial network structure in the base film, further improving the strength and toughness of the base film. DETAILED DESCRIPTION

[0040] The present application is further described in detail below in conjunction with embodiments.

[0041] The raw materials include but are not limited to the following materials: PP is K8003 PP of Shanghai Secco Petrochemical Co., Ltd.; PET is FG600 PET of Ningbo Rongji New Material Technology Co., Ltd.; carbon nanotubes are CNTs of Shanghai Lishuo Composite Materials Co., Ltd.; SiO2 is VN3 industrial grade SiO2 of Degussa (Qingdao) Co., Ltd.; KH550 is KH550 of Shanghai Chuangdao New Materials Co., Ltd.; KH560 is KH560 of Shanghai Sanrong Chemical Technology Co., Ltd.

[0042] Preparation Example

[0043] Preparation example of rare earth modified carbon nanotubes

[0044] Preparation Example 1

[0045] The carbon nanotubes are configured into a dispersion with a mass fraction of 20% (deionized water is used as the solvent), a rare earth compound (lanthanum oxide) is added to the dispersion to make the ion concentration of the rare earth compound in the dispersion 4%, the pH is adjusted to 8 (NaOH adjustment) to obtain a suspension, a flocculant (ammonia water with a mass fraction of 5%) is added to the suspension, and precipitation is carried out at 30°C. The solid matter is retained, washed with ethanol, and vacuum dried to obtain rare earth modified carbon nanotubes.

[0046] Preparation Example 2

[0047] The carbon nanotubes are configured into a dispersion with a mass fraction of 20% (deionized water is used as the solvent), a rare earth compound (lanthanum oxide) is added to the dispersion to make the ion concentration of the rare earth compound in the dispersion 5%, the pH is adjusted to 9 (NaOH adjustment), and a suspension is obtained. A flocculant (ammonia water with a mass fraction of 5%) is added to the suspension, and the suspension is precipitated at 30°C, centrifuged, and the solid matter is retained, washed with ethanol, and vacuum dried to obtain rare earth modified carbon nanotubes.

[0048] Preparation Example 3

[0049] The carbon nanotubes are configured into a dispersion with a mass fraction of 20% (deionized water is used as the solvent), a rare earth compound (lanthanum oxide) is added to the dispersion to make the ion concentration of the rare earth compound in the dispersion 6%, the pH is adjusted to 9 (NaOH adjustment) to obtain a suspension, a flocculant (ammonia water with a mass fraction of 5%) is added to the suspension, and precipitation is carried out at 30°C. The solid matter is retained, washed with ethanol, and vacuum dried to obtain rare earth modified carbon nanotubes.

[0050] Preparation example of carbon nanotubes modified with silk fibroin

[0051] Preparation Example 4

[0052] The silk cocoons were cut into pieces, soaked in a sodium carbonate solution with a mass fraction of 5% for 30 minutes, and degummed, and the process was repeated twice to obtain silk fibroin. The degumming temperature was 100°C, and then the degummed silk fibers were washed 4 times with 1000 mL of deionized water to remove the sericin, and then dried at 45°C for 12 hours to obtain degummed silk fibroin fibers.

[0053] 1 g of carbon nanotubes was dispersed in 80 g of 85% by mass phosphoric acid solution, and ultrasonically mixed for 30 min to obtain a suspension. 8 g of degummed silk fibroin fibers were added to the suspension, homogenized at 8000 rpm for 3 min, centrifuged, the solid matter was retained, and dried to obtain silk fibroin-modified carbon nanotubes.

[0054] Silane coupling agent preparation example

[0055] Preparation Example 5

[0056] Take 0.5 kg KH-550 and 0.5 kg KH-560, add them into a container under a nitrogen atmosphere, stir, heat to 130° C., react for 5 hours, and cool to room temperature to obtain a silane coupling agent.

[0057] Silicon dioxide preparation example

[0058] Preparation Example 6

[0059] Ethanol and water were added to a container in a ratio of 9:1, and the pH value was adjusted to about 4 by adding hydrochloric acid. The silane coupling agent prepared in Preparation Example 5 was added to the container to prepare a solution with a mass fraction of 2%. The solution was stirred at 50°C for 5 hours to obtain a hydrolyzate.

[0060] Add silica to the hydrolyzate, wherein the mass ratio of the silane coupling agent to silica is 1:9, heat the mixed solution to 60°C, stir and mix thoroughly (stirring speed is 500-600r / min) for 5 hours to obtain a modified solution, transfer the modified solution to a tray, and place the tray in an electric blast drying oven, adjust the drying oven temperature to 80°C, dehydrate and dry for 24 hours, and the obtained product is fully crushed to obtain modified silica.

[0061] Example

[0062] Examples 1-3

[0063] In a first aspect, the present application provides a composite current collector heat-resistant base film, comprising the following materials: PP, PET and filler, wherein the filler comprises carbon nanotubes.

[0064] In a second aspect, the present application provides a method for preparing a composite current collector heat-resistant base film, comprising the following steps:

[0065] S1. Raw material blending: PP and PET were placed in an oven at 70°C and dried for 12 hours, and then PP, PET and filler were mixed and melted at 255°C to obtain a PP / PET mixed resin melt;

[0066] S2, melt extrusion: add the PP / PET intermixed resin melt into an extruder (the temperature of the extruder is set to: zone 1 temperature is 235°C, zone 2 temperature is 245°C, zone 3 temperature is 255°C, zone 4 temperature is 265°C, zone 5 temperature is 275°C, and die head temperature is 265°C), heat and melt again, and extrude through granulation to obtain a mixed masterbatch, which reaches the die head after passing through a metering pump, a filter, and an adapter to form a thick sheet;

[0067] S3. Stretching: After the thick sheet is stretched longitudinally, it is stretched transversely, wherein the longitudinal stretching ratio is 1 and the transverse stretching ratio is 3.5, so as to obtain a heat-resistant base film.

[0068] In a third aspect, the present application provides an application of a heat-resistant base film for a composite current collector, and the heat-resistant base film for a composite current collector is applied to a composite current collector.

[0069] Table 1 Composition of heat-resistant base film of Examples 1-3

[0070] Weight / kg Example 1 Example 2 Example 3 PP 90 80 50 PET 10 20 50 filler 0.1 2 10

[0071] Example 4

[0072] The difference from Example 2 is that the filler includes 1 kg of carbon nanotubes and 1 kg of silicon dioxide.

[0073] Example 5

[0074] The difference from Example 2 is that the filler includes 2 kg of rare earth modified carbon nanotubes prepared in Preparation Example 1.

[0075] Example 6

[0076] The difference from Example 2 is that the filler includes 2 kg of rare earth modified carbon nanotubes prepared in Preparation Example 2.

[0077] Example 7

[0078] The difference from Example 2 is that the filler includes 2 kg of rare earth modified carbon nanotubes prepared in Preparation Example 3.

[0079] Example 8

[0080] The difference from Example 2 is that the filler includes 2 kg of silk fibroin-modified carbon nanotubes prepared in Preparation Example 4.

[0081] Example 9

[0082] The difference from Example 2 is that the filler includes 1 kg of rare earth modified carbon nanotubes prepared in Preparation Example 2 and 1 kg of silk fibroin modified carbon nanotubes prepared in Preparation Example 4.

[0083] Example 10

[0084] The difference from Example 4 is that the filler includes 1 kg of carbon nanotubes and 1 kg of modified silica prepared in Preparation Example 6.

[0085] Embodiment 11

[0086] The difference from Example 2 is that the heat-resistant base film is subjected to surface corona treatment using a low-temperature plasma power supply (voltage of 50 V) for 1 min.

[0087] Comparative Example

[0088] Comparative Example 1

[0089] The difference between this comparative example and Example 2 is that no filler is added in this comparative example.

[0090] Comparative Example 2

[0091] The difference between this comparative example and Example 2 is that in this comparative example, an equal mass of POE-g-GMA compatibilizer with a content of 99% produced by Jiangsu Runfeng Synthetic Technology Co., Ltd. is used to replace the filler in Example 2.

[0092] Performance testing

[0093] (1) Tensile property test: This test is performed according to the plastic tensile test method of GB1040-79. The tensile rate is set at 10 mm / min and the heat-resistant film is stretched to break.

[0094] (2) Adhesion performance test: Copper was magnetron sputtered on the heat-resistant film prepared in Example 1-11 and Comparative Example 1-2 to form a 0.2 mm copper plating layer on the heat-resistant film. An adhesion / peeling test was performed using 3M tape, and the number of peeling times was recorded.

[0095] Table 2 Performance test

[0096]

[0097] Combining the performance test comparison in Table 2, we can find that:

[0098] 1. By comparing Examples 1-3 with Comparative Examples 1-2, it can be found that the tensile strength and elongation at break of the heat-resistant base film prepared in Examples 1-3 are both improved, which shows that in the present application, carbon nanotubes are added to the base film. Carbon nanotubes have an excellent aspect ratio and can not only serve as reinforcing particles to improve the strength of the base film, but also reduce the Tg difference between PP and PET and improve the compatibility between PP and PET. Carbon nanotubes can pull at the interface between PP and PET, reduce the sea island structure formed between PP and PET, play a role in increasing volume, and improve the interface bonding effect between PP and PET, thereby improving the tensile effect and strength of the base film. The compatibility of PP and PET can be improved without adding a compatibilizer to the base film, which reduces the possibility of uneven base film strength caused by the migration of small molecules of the compatibilizer, so that the base film obtains uniform strength.

[0099] 2. By comparing Examples 5-7 with Example 2, it can be found that the tensile strength and elongation at break of the heat-resistant base film prepared in Examples 5-7 are improved. This shows that in the present application, the rare earth compound and the carbon nanotubes are ion-bonded through electrostatic attraction, and then stabilized on the surface of the carbon nanotubes by a flocculant to form a coating structure, that is, a core-shell structure, which can reduce the agglomeration of the carbon nanotubes and make the carbon nanotubes evenly dispersed in the base film; at the same time, it can also improve the compatibility of the carbon nanotubes and PP, stabilize and toughen the base film, and improve the strength of the base film.

[0100] 3. By comparing Examples 8-9 with Example 2, it can be found that the tensile strength, elongation at break and adhesion of the heat-resistant base film prepared in Examples 8-9 are all improved, which shows that the silk fibroin used in this application can form a strong π-π interaction with the surface of the carbon nanotubes, so that the carbon nanotubes are evenly dispersed in the base film. Phosphoric acid is used as the dispersion liquid. First, due to the strong polarity of phosphoric acid, the carbon nanotubes can be fully dispersed in phosphoric acid; secondly, the silk fibroin fibers can be quickly dissolved and decomposed in phosphoric acid, so that the silk fibroin can be fully loaded on the carbon nanotubes. At the same time, due to the large number of polar groups in the silk fibroin, it can have a better binding effect with copper ions, that is, improve the binding between the base film and the metal layer.

[0101] 4. By comparing Example 4, Example 10 and Example 2, it can be found that the tensile strength and elongation at break of the heat-resistant base film prepared in Example 10 are both improved, which shows that the use of silica as a filler in the present application can effectively fill the base film and introduce anchoring sites in the base film, thereby improving the bonding effect of PP and PET. The addition of cellulose can use the fiber structure to pull the components in the base film, thereby improving the bonding strength of PP and PET. KH-550 and KH-560 can form a network structure, which is loaded with multiple alkoxy groups and can be combined with the active hydroxyl groups on the surface of silica to achieve grafting modification of silica, so that the silica particles form a structure that is connected but not directly in contact, thereby prompting silica to form a spatial network structure in the base film, further improving the strength and toughness of the base film.

[0102] 5. By comparing Example 11 with Example 2, it can be found that the adhesion of the heat-resistant base film prepared in Example 11 is improved, which means that the corona treatment of the heat-resistant base film in the present application can form a rough structure on the surface of the heat-resistant base film and improve the bonding strength between the heat-resistant base film and the metal layer.

[0103] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A composite current collector heat-resistant base film, characterized in that: The materials include the following parts by weight: PP 50-99 copies; PET 1-50 parts; The filler comprises 0.1-10 parts of carbon nanotubes; the carbon nanotubes comprise carbon nanotubes modified by silk fibroin, and the preparation of the carbon nanotubes modified by silk fibroin comprises: dispersing the carbon nanotubes in a phosphoric acid solution, ultrasonically mixing to obtain a suspension, adding degummed silk fibroin fibers to the suspension, homogenizing, centrifuging, retaining solids, and drying to obtain the silk fibroin modified carbon nanotubes.

2. The method for preparing a heat-resistant composite current collector base film according to claim 1, characterized in that: The following steps are involved: S1. Raw material blending: PP, PET and filler are mixed and heated to melt to obtain PP / PET mixed resin melt; S2, melt extrusion: PP / PET intermixed resin melt is granulated and extruded to obtain mixed masterbatch, which is heated and melted again, and reaches the die head to form a thick sheet after passing through a metering pump, a filter, and an adapter; S3. Stretching: After the thick sheet is stretched longitudinally, it is stretched transversely to obtain a heat-resistant base film.

3. The method for preparing a composite current collector heat-resistant base film according to claim 2, characterized in that: The heat-resistant base film is subjected to corona treatment.

4. An application of a composite current collector heat-resistant base film, characterized in that: The heat-resistant base film for composite current collector described in claim 1 is applied to the composite current collector.