A short-process preparation device for fine-grained tungsten ingots
Through the combination of plasma melting electrodes and gas jet refining droplets, permanent magnet speed bumps and cooling devices, combined with ultrasonic vibration, the problems of high impurities, long processes and coarse grains in the preparation of tungsten ingots are solved, and the production of tungsten ingots is achieved. The short-process preparation achieves a fine-grained structure with low impurities and high density.
Patent Information
- Application Number
- CN202211006324.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-22
AI Technical Summary
When preparing tungsten ingots in the prior art, there are problems such as high impurities, long process routes, and coarse grains.
The plasma melting electrode is used to melt the tungsten material into droplets, and the droplets are refined through the gas blowing device. The permanent magnetic deceleration belt is used to reduce the falling speed. The cooling device and the ultrasonic vibration device are combined to realize the short-process preparation of tungsten ingots and control the temperature. and solidification process to obtain fine-grained structure and high density.
It effectively reduces the impurity content of tungsten ingots, shortens the process route, and forms fine-grained structure and high-density tungsten ingots, which is superior to powder metallurgy and arc melting methods and is suitable for subsequent thermal processing.
Smart Images

Figure CN115889775B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal smelting, and in particular to a short-process preparation device for fine-grained tungsten ingots. Background Art
[0002] Tungsten, a refractory metal, has been widely used in aerospace, military, nuclear power and other fields due to its extremely high melting point and high temperature strength. In these application fields, most tungsten products are prepared by powder metallurgy billets combined with subsequent hot processing and mechanical processing. The metallurgical quality of powder metallurgy billets determines the service performance, processing yield, processing technology, etc. of tungsten products prepared by subsequent processing procedures. Therefore, for the preparation of tungsten products, the most important process is to obtain a good billet metallurgical quality. Among them, the most important indicator of billet metallurgical quality is the grain size of the tungsten ingot. The finer the grain size of the tungsten billet, the better its processing technology and the higher the processing yield. In addition, the purity of the tungsten billet also significantly affects the processing technology of the billet and the service performance of the final product. The higher the purity of the billet, the better the plasticity of the final tungsten product and the higher its ductile-brittle transition temperature.
[0003] In order to obtain fine-grained tungsten ingots, the commonly used method is to hot-press ultrafine tungsten powder into tungsten ingots by powder metallurgy. However, this preparation method easily introduces impurities such as C, N, and O, which seriously deteriorates the performance of the tungsten ingot, especially reduces the plastic-brittle transition temperature of tungsten. Moreover, for powder metallurgy, its process flow generally includes: preparing high-purity tungsten oxide powder → reducing tungsten oxide powder to pure tungsten powder → screening pure tungsten powder to obtain pure tungsten powder of the required particle size → mixing pure tungsten powder and cold pressing into billets → sintering the cold pressed tungsten billets at high temperature. The sintering process is not only time-consuming and energy-consuming, but also requires high equipment costs. This preparation method has a long processing flow and high costs. In addition, in order to obtain high-purity tungsten ingots during production, arc melting is generally used to prepare tungsten ingots. During the arc melting process, due to the extremely high vacuum degree and the strong evaporation effect of the arc, the impurities such as C, N, and O originally present in the tungsten material can be evaporated to prepare high-purity tungsten ingots. However, the grains of tungsten ingots prepared by arc melting are very coarse, which is not conducive to the subsequent heat processing process. Summary of the invention
[0004] The present invention provides a short-process preparation device for fine-crystal tungsten ingots, which can solve the problems of high impurities, long process route and coarse grains in the preparation of tungsten ingots in the prior art.
[0005] A short-process preparation device for fine-grained tungsten ingots, comprising a base and:
[0006] The plasma melting electrode is arranged on the side of the tungsten material and is used to melt the tungsten material into liquid droplets and drip them under the action of gravity;
[0007] A gas blowing device, arranged on the moving track of the liquid droplets under the action of gravity, for blowing an inert gas to the liquid droplets to refine the liquid droplets;
[0008] A permanent magnetic speed reduction belt is used to reduce the falling speed of the refined droplets; and,
[0009] The cooling device is used to cool the tungsten ingot formed by dripping onto the base through the permanent magnetic speed reduction belt.
[0010] More preferably, the base has a first water inlet and a first water outlet for introducing a cooling medium to cool the base.
[0011] More preferably, the cooling device includes a cooling body, a second water inlet and a second water outlet, the cooling body is arranged around the circumference of the base, and the second water inlet and the second water outlet are both opened on the cooling body for passing cooling medium to absorb the radiant heat of the tungsten ingot.
[0012] More preferably, it also includes a controller, a water supply device and a non-contact temperature measuring device;
[0013] The non-contact temperature measuring device and the water supply device are both connected to the controller by signal, the non-contact temperature measuring device is used to monitor the temperature of the tungsten ingot, and the controller is used to control the operation of the water supply device according to the temperature; wherein,
[0014] The water supply device is connected to the base and the cooling device.
[0015] More preferably, it further comprises an ultrasonic vibration device, which is arranged on the substrate and is used to make the tungsten ingot generate high-frequency vibration.
[0016] More preferably, the frequency of the high-frequency vibration is 2000-5000HZ.
[0017] More preferably, the gas blowing device is 40 mm away from the plasma melting electrode.
[0018] More preferably, the permanent magnetic speed reduction belt has a length of 20 to 30 cm.
[0019] More preferably, the gas pressure formed by the gas blowing device is 2 MPa.
[0020] The present invention provides a short-process preparation device for fine-crystalline tungsten ingots, which can achieve at least one of the following beneficial effects:
[0021] 1. By using plasma melting electrodes, the impurity content of tungsten ingots is low;
[0022] 2. Through the gas blowing device and controlled liquid phase accumulation, the smelting and solidification of tungsten ingots are completed in one process, realizing the short process preparation of tungsten ingots, avoiding the disadvantage of long process of powder metallurgy, and the tungsten ingot structure is fine-grained, which is better than the ultra-large grain structure of conventional arc melting;
[0023] 3. By online controlling the solidification heat dissipation intensity of the tungsten ingot during solidification and supplemented by ultrasonic vibration, on the one hand, the microstructure refinement process during the solidification of the tungsten ingot is promoted, and on the other hand, the density of the tungsten ingot is improved, so that the prepared tungsten ingot has both fine-grained structure and high density, which is beneficial to the subsequent thermal processing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of the structure of a short-process preparation device for fine-grained tungsten ingots provided by the present invention;
[0025] Figure 2 A metallographic structure diagram of a tungsten ingot prepared by a short-process preparation device for a fine-crystal tungsten ingot according to the present invention;
[0026] Figure 3 This is the metallographic structure diagram of the original powder metallurgy tungsten ingot;
[0027] Figure 4 This is the metallographic structure diagram of arc-melted tungsten ingot (scale 1 cm).
[0028] Description of reference numerals:
[0029] 10 plasma melting electrode; 11 gas blowing device; 12 permanent magnetic speed reduction belt; 13 infrared temperature measuring probe; 14 cooling body; 141 second water inlet; 142 second water outlet; 15 base; 16 ultrasonic vibration device; 20 tungsten material; 21 molten droplet area; 22 ultrafine droplet area; 23 tungsten ingot. DETAILED DESCRIPTION
[0030] A specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation.
[0031] Embodiment 1:
[0032] like Figure 1 As shown, the present invention provides a short-process preparation device for a fine-grained tungsten ingot 23, which includes a plasma melting electrode 10, a gas blowing device 11, a permanent magnetic speed reduction belt 12, a cooling device and a base 15 arranged in sequence from top to bottom.
[0033] The plasma melting electrode 10 is arranged on the side of the tungsten material 20, and is used to generate high temperature to melt the tungsten material 20 into liquid droplets and drip under the action of gravity. A tungsten ingot 23 with high impurity content or unqualified grain size, or a waste tungsten material 20 after surface purification treatment is placed on the base 15. In this embodiment, a powder metallurgy tungsten ingot 23 is used as the tungsten material 20 as an example. The plasma arc is very suitable for melting tungsten because it can easily generate a high temperature of more than 4000°C. Its melting principle is similar to arc melting, and the gas between the electrode and the workpiece is ionized to form a plasma state, thereby melting the tungsten material 20. However, during smelting, the plasma melting electrode 10 can be located on the side of the tungsten material 20, thereby allowing the liquid tungsten to fall freely under the action of gravity instead of falling on the electrode, providing a basis for further producing ultrafine droplets by blowing high-pressure gas generated by the gas blowing device 11. In general arc melting, the original tungsten material 20 is used as the anode and the tungsten material 20 after melting and solidification is used as the cathode. The two are located in the upper and lower positions in space. Therefore, after the liquid tungsten is produced by conventional arc melting, it can only fall on the tungsten material 20 below. The distance between the two is generally only about 2 mm. With such a short falling distance, it is impossible to carry out the high-pressure gas blowing atomization process of the liquid tungsten.
[0034] The gas blowing device 11 is arranged on the moving track of the droplets under the action of gravity, and is used to blow inert gas to the droplets to refine the droplets. After the plasma smelting produces liquid tungsten, the gas blowing device 11 is arranged on the free fall path of the liquid tungsten, about 40 mm away from the plasma melting electrode 10, and is used to blow high-pressure inert gas, and the gas pressure is 2MPa, so that the liquid tungsten can be blown into ultrafine droplets, and then the ultrafine droplets are mixed with the inert gas to form a gas-liquid mixture and fall at a high speed. The inert gas can form a protective atmosphere to prevent the high-temperature liquid tungsten from being oxidized.
[0035] As can be seen from the above, the melted liquid tungsten is roughly divided into two sections. When the tungsten material 20 is melted under the action of the plasma melting electrode 10, liquid tungsten is formed and falls freely under the action of gravity. This falling process is the melting droplet zone. The liquid particles of the liquid tungsten in this section are relatively large. When the liquid tungsten continues to fall to the position of the gas blowing device 11, the liquid tungsten is blown into ultrafine droplets under the blowing of high-pressure gas and falls through the permanent magnetic speed reduction belt 12. This section is the ultrafine droplet zone 22.
[0036] The permanent magnetic speed reduction belt 12 is annular, and can be specifically an annular magnet, which is used to generate a permanent magnetic field, cover the ultrafine droplet area 22, and reduce the falling speed of the refined droplets. Liquid tungsten has a very high speed because it is mixed with high-pressure gas, so it is not suitable for direct stacking and forming, and the liquid tungsten needs to be slowed down first. Since tungsten is a conductor, a permanent magnetic field can be used to slow down. When liquid tungsten passes through a permanent magnetic field, it is actually a process in which a conductor cuts magnetic flux lines, so an electric field is generated in the liquid tungsten, and the electric field generates an induced current, and the current generates a magnetic field opposite to the original permanent magnetic field. Therefore, the interaction of the two magnetic fields will cause the liquid tungsten to slow down rapidly. Although the liquid tungsten is very fast, the droplets are very small, so the weight is small, and it only needs to pass through a permanent magnetic field of about 20-30cm in length to slow down to a speed suitable for stacking and forming.
[0037] The cooling device is used to cool the tungsten ingot 23 formed by dripping onto the base 15 through the permanent magnetic speed reduction belt 12. After the mixture of inert gas and liquid tungsten is decelerated by the permanent magnetic speed reduction belt 12, the liquid tungsten can be formed on the substrate by continuous stacking. During the forming process, the liquid tungsten begins to solidify when it touches the substrate. In this process, the solidification of the liquid tungsten will generate a large amount of latent heat of solidification. This part of heat must be conducted away to ensure the smooth solidification of the subsequent tungsten droplets.
[0038] There are two main ways to conduct away heat. In one scheme, the base has a cavity structure, and the base 15 has a first water inlet and a first water outlet for introducing a cooling medium to cool the base 15. Cooling water or other cooling medium is introduced into the cavity of the base 15, and the cooling water cools the base and then cools the tungsten ingot 23 accumulated on the base. In another scheme, in addition to cooling the base, the thermal radiation of the tungsten ingot 23 is also absorbed and cooled. By arranging a water-permeable copper sleeve around the tungsten ingot 23, the copper sleeve has a second water inlet 141 and a second water outlet 142, and the copper sleeve is arranged on the peripheral side of the tungsten ingot 23, the thermal radiation heat dissipation process of the tungsten ingot 23 can be strengthened. Through these two ways, the purpose of conducting away the latent heat of solidification generated by cooling the liquid tungsten can be fully met.
[0039] C content N content O content Raw powder metallurgy tungsten ingot 500ppm 300ppm 700ppm Reshaping Tungsten Ingot 100ppm 25ppm 35ppm
[0040] Table 1
[0041] Table 1 shows the C, N, and O contents of the tungsten ingot 23 prepared in this embodiment and the original powder metallurgy tungsten ingot 23. It can be seen from the table that the impurity content of the original powder metallurgy tungsten ingot 23 is greatly reduced after being reshaped by the device of the present invention, which fully demonstrates the beneficial effect of the present invention in effectively removing impurities.
[0042] Embodiment 2:
[0043] On the basis of embodiment 1, it also includes a controller, a water supply device and a non-contact temperature measuring device. In this embodiment, the non-contact temperature measuring device adopts an infrared temperature measuring probe 13. It can be understood that other non-contact temperature detection devices can also be used; wherein the water supply device is a water pump with a water pressure regulating function.
[0044] The infrared temperature probe 13 and the water supply device are both connected to the controller. The infrared temperature probe 13 is used to monitor the temperature of the tungsten ingot 23. The controller is used to control the operation of the water supply device according to the temperature to adjust the water pressure. The water supply device is connected to the base 15 and the cooling device.
[0045] In the process of the liquid tungsten solidifying into the solid phase tungsten ingot 23, the top temperature of the solid phase tungsten ingot 23 determines the difficulty of the liquid tungsten stacking on the surface of the tungsten ingot 23. If the temperature of the tungsten ingot 23 is low, the liquid tungsten solidifies quickly on the surface of the tungsten ingot 23, which is easy to produce the defects of insufficient stacking density and high porosity of the tungsten ingot 23. If the temperature of the tungsten ingot 23 is high, it is easy to produce the disadvantages of slow cooling of the liquid tungsten and coarse structure of the tungsten ingot 23. Therefore, it is necessary to set an infrared temperature probe 13 on the side of the tungsten ingot 23, and send the temperature of the upper surface of the tungsten ingot 23 as a feedback signal to the controller, and the controller controls the water supply device in real time to adjust the water pressure of the cooling water in the base and the copper sleeve around the tungsten ingot 23, and then adjust the cooling intensity of the tungsten ingot 23, so as to adjust the temperature of the upper surface of the tungsten ingot 23 in real time, achieve the best metallurgical quality of the tungsten ingot 23, and make the tungsten ingot 23 have good density and fine grain structure. Specifically, in this embodiment, the top temperature of the tungsten ingot 23 is controlled at 3000°C to 3200°C.
[0046] Embodiment three:
[0047] On the basis of the first or second embodiment, when the liquid tungsten falls on the upper surface of the tungsten ingot 23 and solidifies, in order to refine the solidification structure of the tungsten ingot 23 and improve the density, this embodiment also sets an ultrasonic vibration device 16 on the substrate. On the one hand, the ultrasonic vibration can break up the grains in the liquid tungsten solidification process to produce the effect of tissue refinement. On the other hand, the vibration can also promote the fluidity of the liquid phase on the upper surface of the tungsten ingot 23, thereby promoting the liquid phase to fill the holes caused by insufficient stacking, thereby improving the density of the tungsten ingot 23.
[0048] The density of the sample was indirectly measured by the Archimedes method. The density of the tungsten ingot 23 prepared by the powder metallurgy method and the tungsten ingot 23 prepared by the arc melting method purchased from Nangong Ruili Alloy Welding Material Co., Ltd. and the tungsten ingot 23 prepared by the preparation method provided by the present invention were measured, and the test results are as follows:
[0049] The density of the powder metallurgy tungsten ingot 23 is 90%-95%, the density of the arc melting tungsten ingot 23 is 99%-100%, and the density of the invention of the present application is 99%-100%.
[0050] It can be seen that the density of the tungsten ingot 23 prepared by the preparation method provided by the present invention is higher than that of the tungsten ingot 23 prepared by the powder metallurgy method, and is equivalent to that of the tungsten ingot 23 prepared by the arc melting method.
[0051] In this embodiment, the vibration frequency of the ultrasonic vibration device 16 is 2000-5000 Hz, preferably 3000 Hz, which can achieve the dual effects of good billet structure refinement and density improvement.
[0052] Figure 2 The metallographic structure diagram of the original powder metallurgy tungsten ingot 23 is shown. Figure 3 The metallographic structure diagram of the tungsten ingot 23 prepared by the device of the present invention is shown. Figure 4 The metallographic structure diagram of the arc-melted tungsten ingot 23 is shown. As can be seen from the figure, the structure of the tungsten ingot 23 produced by the device of the present invention is equivalent to the structure of the powder metallurgy tungsten billet, but the device of the present invention saves the complicated powder metallurgy process in preparing the billet. Compared with the metallographic structure of the arc-melted tungsten ingot 23, the billet grains prepared by the method of the present invention are smaller.
[0053] The above disclosures are only several specific embodiments of the present invention. However, the embodiments of the present invention are not limited thereto. Any changes that can be conceived by those skilled in the art should fall within the protection scope of the present invention.
Claims
1. A short-process preparation device for fine-grained tungsten ingots, comprising a base (15), characterized in that: Also includes: A plasma melting electrode (10) is arranged on the side of the tungsten material (20) and is used to melt the tungsten material (20) into liquid droplets and drip them under the action of gravity; A gas blowing device (11), arranged on the moving track of the liquid droplets under the action of gravity, for blowing an inert gas to the liquid droplets to refine the liquid droplets; A permanent magnetic speed reduction belt (12) is used to reduce the falling speed of the refined droplets; and A cooling device for cooling the tungsten ingot (23) formed by dripping onto the base (15) through the permanent magnetic speed reduction belt (12); The base (15) has a first water inlet and a first water outlet, which are used to allow a cooling medium to flow in to cool the base (15); The cooling device comprises a cooling body (14), a second water inlet (141) and a second water outlet (142); the cooling body (14) is arranged around the circumference of the base (15); the second water inlet (141) and the second water outlet (142) are both provided on the cooling body (14) for passing a cooling medium to absorb the radiant heat of the tungsten ingot (23); It also includes a controller, a water supply device and a non-contact temperature measurement device; The non-contact temperature measuring device and the water supply device are both connected to the controller by signal, the non-contact temperature measuring device is used to monitor the temperature of the tungsten ingot (23), and the controller is used to control the operation of the water supply device according to the temperature; wherein, The water supply device is connected to the base (15) and the cooling device; It also includes an ultrasonic vibration device (16), which is arranged on the base (15) and is used to make the tungsten ingot (23) generate high-frequency vibration; The frequency of the high-frequency vibration is 2000-5000HZ.
2. A short-process preparation device for fine-grained tungsten ingots as claimed in claim 1, characterized in that: The gas blowing device (11) is 40 mm away from the plasma melting electrode.
3. A short-process preparation device for fine-crystalline tungsten ingots as claimed in claim 1, characterized in that: The permanent magnetic speed reduction belt (12) has a length of 20 to 30 cm.
4. A short-process preparation device for fine-crystalline tungsten ingots as claimed in claim 1, characterized in that: The gas pressure formed by the gas blowing device (11) is 2 MPa.
Citation Information
Patent Citations
Processes, systems, and apparatus for forming products from atomized metals and alloys
CN103747898A
Metal micro-spraying molten drop electromagnetic restraint deposition modeling system
CN104028761A