A modified carbon nanotube and a preparation method thereof, a graphite bipolar plate and a preparation method thereof

Modified carbon nanotubes are prepared by curing and pyrolysis methods of phenolic resin, metal salt catalyst and alcohol solvent, which improves the strength and conductivity of graphite bipolar plates, solves the problem of low strength of graphite bipolar plates, and achieves more efficient Forming and mass production.

CN115893378BActive Publication Date: 2024-11-12HAIDRIVER (BEIJING) ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211437486.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-11-12
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

The existing graphite bipolar plates have low strength due to poor compatibility with graphite, which limits their application.

Method used

Modified carbon nanotubes were prepared by mixed curing and pyrolysis methods of phenolic resin, metal salt catalyst and alcohol solvent to improve their compatibility with graphite, and graphite bipolar plates were obtained through tapping and cold pressing molding.

Benefits of technology

The strength and conductivity of graphite bipolar plates are improved, the forming process is simplified, and the difficulty of large-scale production is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115893378B_ABST
    Figure CN115893378B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of fuel cell technology, and provides a modified carbon nanotube and a preparation method thereof, a graphite bipolar plate and a preparation method thereof. The preparation method provided by the present invention mixes a phenolic resin, a catalyst and an alcohol solvent, and sequentially solidifies and pyrolyzes them to obtain the modified carbon nanotube; the catalyst is a metal salt. The present invention uses a metal salt as a catalyst to crack the cured phenolic resin into carbon nanotubes, and the obtained carbon nanotubes have graphite knots, which improves its compatibility with graphite, thereby improving the strength and conductivity of the graphite bipolar plate. The data of the embodiment show that the conductivity of the obtained graphite bipolar plate is 579-620S / cm, and the bending strength is 75-102MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fuel cells, and in particular to a modified carbon nanotube and a preparation method thereof, a graphite bipolar plate and a preparation method thereof. Background Art

[0002] As the core component of fuel cells, bipolar plates have received extensive attention. Among them, metal bipolar plates and graphite bipolar plates are commonly used. Metal bipolar plates have the disadvantages of being easily corroded and high in cost under acidic conditions. In comparison, graphite bipolar plates have the advantages of high conductivity, corrosion resistance and low cost. The existing method for preparing graphite bipolar plates is to use graphite, a curing agent and carbon nanotubes as raw materials, and prepare them by a prefabricated plate method or a powder molding method. However, the existing carbon nanotubes have poor compatibility with graphite, resulting in low strength of the resulting graphite bipolar plates, which restricts the application of graphite bipolar plates. Summary of the invention

[0003] In view of this, the object of the present invention is to provide a modified carbon nanotube and a preparation method thereof, a graphite bipolar plate and a preparation method thereof. The modified carbon nanotube obtained by the preparation method provided by the present invention has good compatibility with graphite, thereby improving the strength of the graphite bipolar plate.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing modified carbon nanotubes, comprising the following steps:

[0006] Mixing phenolic resin, a catalyst and an alcohol solvent, and sequentially curing and pyrolyzing them to obtain the modified carbon nanotubes;

[0007] The catalyst is a metal salt.

[0008] Preferably, the metal salt comprises metal nitrate or ferrocene; the metal nitrate comprises one or more of ferric nitrate, nickel nitrate, manganese nitrate and cobalt nitrate.

[0009] Preferably, the mass of the metal salt is 0.25-1% of the mass of the phenolic resin.

[0010] Preferably, the alcohol solvent includes one or more of isopropanol, butanediol and isoprenediol.

[0011] Preferably, the curing comprises sequentially performing a first curing and a second curing;

[0012] The first curing temperature is 70-80°C and the time is 8-12h;

[0013] The second curing temperature is 100-120° C. and the time is 20-24 hours.

[0014] Preferably, the pyrolysis comprises sequentially performing a first pyrolysis and a second pyrolysis;

[0015] The temperature of the first pyrolysis is 300-500°C, the holding time is 20-30min, and the rate of heating to the first pyrolysis temperature is 5°C / min;

[0016] The temperature of the second pyrolysis is 600-1200°C, the holding time is 30-60min, and the rate of increasing from the temperature of the first pyrolysis to the temperature of the second pyrolysis is 1°C / min;

[0017] The pyrolysis is carried out under a protective atmosphere.

[0018] The present invention also provides modified carbon nanotubes obtained by the preparation method described in the above technical solution.

[0019] The present invention also provides a graphite bipolar plate, which is prepared from the following raw materials: graphite and modified carbon nanotubes;

[0020] The modified carbon nanotubes are the modified carbon nanotubes described in the above technical solution;

[0021] The mass of the modified carbon nanotubes is 1-10% of the mass of the graphite.

[0022] The present invention also provides a method for preparing the graphite bipolar plate described in the above technical solution, comprising the following steps:

[0023] The graphite and modified carbon nanotubes are mixed, and then subjected to vibration compaction treatment and cold pressing in sequence to obtain the graphite bipolar plate.

[0024] Preferably, the parameters of the vibration treatment include: vibration amplitude of 0.01 to 100 mm, frequency of 1 to 400 times / min, and vibration time of 3 to 5 min;

[0025] The pressure of the cold press molding is programmed pressure increase, and the parameters of the programmed pressure increase include: an initial pressure of 5MPa, a pressure increase rate of 2.5MPa / min, a terminal pressure of 50MPa, and a holding time of the terminal pressure of 10 to 20min.

[0026] The present invention provides a method for preparing modified carbon nanotubes, comprising the following steps: mixing a phenolic resin, a catalyst and an alcohol solvent, and sequentially curing and pyrolyzing to obtain the modified carbon nanotubes; the catalyst is a metal salt. The present invention uses a metal salt as a catalyst to crack the cured phenolic resin into carbon nanotubes, and the obtained carbon nanotubes have graphite knots, which improves its compatibility with graphite, thereby improving the strength and conductivity of the graphite bipolar plate. The data of the embodiment show that the conductivity of the obtained graphite bipolar plate is 579-620S / cm, and the bending strength is 75-102MPa.

[0027] The present invention also provides modified carbon nanotubes obtained by the preparation method described in the above technical solution. The modified carbon nanotubes provided by the present invention have high fusion property with graphite.

[0028] The present invention also provides a graphite bipolar plate, which is prepared from the following raw materials: graphite and modified carbon nanotubes; the modified carbon nanotubes are the modified carbon nanotubes described in the above technical solution; the mass of the modified carbon nanotubes is 1-10% of the mass of the graphite. Since the graphite bipolar plate provided by the present invention uses modified carbon nanotubes, the graphite bipolar plate has good strength and conductivity.

[0029] The present invention also provides a method for preparing the graphite bipolar plate described in the above technical solution, comprising the following steps: mixing graphite and modified carbon nanotubes, performing vibration treatment and cold pressing in sequence, to obtain the graphite bipolar plate. The preparation method of the present invention uses modified carbon nanotubes, and since the modified carbon nanotubes have good compatibility with graphite, the difficulty of cold pressing is reduced; at the same time, compared with the existing prefabricated plate method or powder molding method, the molding process is faster, the molding rate of the obtained graphite bipolar plate is higher, and it is easier to achieve large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a transmission electron microscope photo of the modified carbon nanotubes obtained in Example 1;

[0031] Figure 2 This is a transmission electron microscope photograph of the modified carbon nanotubes obtained in Example 3. DETAILED DESCRIPTION

[0032] The present invention provides a method for preparing modified carbon nanotubes, comprising the following steps:

[0033] Mixing phenolic resin, a catalyst and an alcohol solvent, and sequentially curing and pyrolyzing them to obtain the modified carbon nanotubes;

[0034] The catalyst is a metal salt.

[0035] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.

[0036] In the present invention, the phenolic resin is preferably of Sumitomo PR55738, Sumitomo PR12603 or Sumitomo PR55147.

[0037] In the present invention, the metal salt preferably includes metal nitrate or ferrocene. In the present invention, the metal nitrate preferably includes one or more of ferric nitrate, nickel nitrate, manganese nitrate and cobalt nitrate. In the present invention, the mass of the metal salt is preferably 0.25-1% of the mass of the phenolic resin, and more preferably 0.5-0.75%.

[0038] In the present invention, the alcohol solvent preferably includes one or more of isopropanol, butanediol and isopentyl glycol. In the present invention, the alcohol solvent and the phenolic resin are preferably used in a ratio of 50-100 mL: 40-80 g.

[0039] In the present invention, the mixing of the phenolic resin, the catalyst and the alcohol solvent preferably comprises: dispersing the catalyst in the alcohol solvent, and then adding the phenolic resin for stirring and mixing. In the present invention, the stirring and mixing speed is preferably 6000-10000 rpm, more preferably 7000-9000 rpm, and more preferably 8000 rpm; the time is preferably 40 min-2 h.

[0040] In the present invention, the curing preferably includes performing first curing and second curing in sequence.

[0041] In the present invention, the first curing temperature is preferably 70 to 80° C., more preferably 75° C.; the first curing time is preferably 8 to 12 hours, more preferably 10 to 11 hours.

[0042] In the present invention, the temperature of the second curing is preferably 100 to 120° C., more preferably 105 to 115° C., and more preferably 110° C.; the time is preferably 20 to 24 hours.

[0043] In the present invention, the pyrolysis is preferably carried out under a protective atmosphere; the protective atmosphere preferably includes argon. In the present invention, the pyrolysis preferably includes sequentially carrying out a first pyrolysis and a second pyrolysis.

[0044] In the present invention, the temperature of the first pyrolysis is preferably 300-500°C, more preferably 350-450°C, and more preferably 400°C; the insulation time is preferably 20-30min, and more preferably 25min; the rate of heating to the first pyrolysis temperature is preferably 5°C / min.

[0045] In the present invention, the temperature of the second pyrolysis is preferably 600-1200°C, more preferably 800-1000°C; the insulation time is preferably 30-60min, more preferably 40-50min, and the rate of increasing the temperature from the first pyrolysis temperature to the second pyrolysis temperature is preferably 1°C / min.

[0046] The present invention also provides a modified carbon nanotube obtained by the preparation method described in the above technical solution. The modified carbon nanotube provided by the present invention has good fusion property with graphite.

[0047] The present invention also provides a graphite bipolar plate, which is prepared from the following raw materials: graphite and modified carbon nanotubes;

[0048] The modified carbon nanotubes are the modified carbon nanotubes described in the above technical solution;

[0049] The mass of the modified carbon nanotubes is 1-10% of the mass of the graphite.

[0050] The raw material for preparing the graphite bipolar plate provided by the present invention includes graphite. In the present invention, the particle size of the graphite is preferably 100-300 mesh. In the present invention, the graphite preferably includes one or more of expanded graphite, microcrystalline graphite and natural flake graphite. In the present invention, the particle size of the expanded graphite is preferably 150-200 mesh; the particle size of the microcrystalline graphite is preferably 200-300 mesh; the particle size of the natural flake graphite is preferably 100-150 mesh.

[0051] The raw materials for preparing the graphite bipolar plate provided by the present invention include modified carbon nanotubes; the modified carbon nanotubes are the modified carbon nanotubes described in the above technical solution. In the present invention, the length of the modified carbon nanotubes is preferably 15 to 25 nm. In the present invention, the mass of the modified carbon nanotubes is preferably 1 to 10% of the mass of the graphite, more preferably 3 to 8%, and more preferably 4 to 6%.

[0052] The present invention also provides a method for preparing the graphite bipolar plate described in the above technical solution, comprising the following steps:

[0053] The graphite and modified carbon nanotubes are mixed, and then subjected to vibration compaction treatment and cold pressing in sequence to obtain the graphite bipolar plate.

[0054] In the present invention, the parameters of the vibration treatment include: the vibration amplitude is preferably 0.01-100 mm, more preferably 50-80 mm; the frequency is preferably 1-400 times / min, more preferably 200-300 times / min; the vibration time is preferably 3-5 min.

[0055] In the present invention, the pressure of the cold press molding is preferably programmed pressure increase, and the parameters of the programmed pressure increase include: the initial pressure is preferably 5MPa, the pressure increase rate is preferably 2.5MPa / min, the end pressure is preferably 50MPa, and the holding time of the end pressure is preferably 10 to 20min.

[0056] In the present invention, the cold pressing molding preferably includes: placing the composite powder after the vibration treatment in a molding cavity and performing programmed pressure increase.

[0057] In the present invention, the mold cavity is preferably coated with a release agent. In the present invention, the release agent preferably includes stearate and / or silicone oil. In the present invention, the stearate preferably includes one or more of zinc stearate, sodium stearate, magnesium stearate and aluminum stearate.

[0058] The modified carbon nanotubes and preparation methods thereof, the graphite bipolar plates and preparation methods thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0059] Example 1

[0060] Weigh 0.1g (0.25% by mass of phenolic resin) nickel nitrate as a catalyst, dissolve it in 50mL of isopropanol, then pour 40g of Sumitomo PR-55738 phenolic resin into it, use a blade stirrer, the stirring rate is 8000rpm, stir evenly for 1h to avoid resin agglomeration, and the obtained dispersion system is first cured at 80°C for 10h, and then cured at 120°C for 24h; in an argon atmosphere, first heat the cured phenolic resin to 300°C at a heating rate of 5°C / min and keep it warm for 30min, then heat it to 600°C at a heating rate of 1°C / min and keep it warm for 40min to obtain modified carbon nanotubes for use.

[0061] Weigh 5g of modified carbon nanotubes (5% of the mass of graphite) and 100g of 150-mesh expanded graphite, place them on a vibration table for compaction treatment, with an amplitude of 50mm, a frequency of 200 times / min, and a vibration time of 3min. Place the compacted material in a molding cavity (zinc stearate is applied to the inside of the molding cavity as a release agent), perform program pressure increase, the initial pressure is 5MPa, the pressure increase rate is 2.5MPa / min, the final pressure is 50MPa, and the pressure is maintained at the final pressure for 10min to obtain a graphite bipolar plate.

[0062] Example 2

[0063] Weigh 0.2g (0.5% by mass of phenolic resin) cobalt nitrate as a catalyst, dissolve it in 50mL of butanediol, then pour 40g of Sumitomo PR-12603 phenolic resin into it, use a blade stirrer, stir at a rate of 6000r / min, stir evenly for 40min to avoid resin agglomeration, and obtain a dispersed system. First cure at 80℃ for 12h, and then cure at 100℃ for 20h; in an argon atmosphere, first heat the cured phenolic resin to 300℃ at a heating rate of 5℃ / min for 30min, then heat it to 800℃ at a heating rate of 1℃ / min for 40min, and obtain modified carbon nanotubes for standby use.

[0064] Weigh 10g of modified carbon nanotubes (10% of the mass of graphite) and 100g of 200-mesh microcrystalline graphite, place them on a vibration table for compaction treatment, with an amplitude of 100mm, a frequency of 400 times / min, and a vibration time of 5min. Place the compacted material in a molding cavity (sodium stearate is applied to the inside of the molding cavity as a release agent), perform program pressure increase, with an initial pressure of 5MPa, a pressure increase rate of 2.5MPa / min, and a final pressure of 50MPa. Maintain the pressure at the final pressure for 15min to obtain a graphite bipolar plate.

[0065] Example 3

[0066] Weigh 0.5g (0.5% by weight of phenolic resin) ferrocene as a catalyst, dissolve it in 60mL isopropanol, then pour 100g of Sumitomo PR-55147 phenolic resin into it, use a blade stirrer, stir at a rate of 10000r / min, stir evenly for 1h to avoid resin agglomeration, and obtain a dispersed system. First cure at 80℃ for 8h, and then cure at 120℃ for 24h; in an argon atmosphere, first heat the cured phenolic resin to 300℃ at a heating rate of 5℃ / min for 30min, then heat it to 1000℃ at a heating rate of 1℃ / min for 40min, and obtain modified carbon nanotubes for use.

[0067] Weigh 10g of modified carbon nanotubes (10% of the mass of graphite), 50g of 200-mesh microcrystalline graphite, and 50g of 150-mesh expanded graphite, and place them on a vibration table for compaction treatment, with an amplitude of 80mm, a frequency of 300 times / min, and a vibration time of 5min. Place the compacted material in a mold cavity (silicone oil is applied to the inside of the mold cavity as a release agent), and perform program pressure increase, with an initial pressure of 5MPa, a pressure increase rate of 2.5MPa / min, and a final pressure of 50MPa. Maintain the pressure at the final pressure for 20min to obtain a graphite bipolar plate.

[0068] Comparative Example 1

[0069] Weigh 5g of commercially available Toray carbon nanotubes with an average length of 100nm (5% of the mass of graphite) and 100g of 150-mesh expanded graphite, place them on a vibration table for compaction treatment, with an amplitude of 50mm, a frequency of 200 times / min, and a vibration time of 3min. Place the compacted material in a molding cavity (zinc stearate is applied to the inside of the molding cavity as a release agent), perform program pressure increase, with an initial pressure of 5MPa, a pressure increase rate of 2.5MPa / min, and a final pressure of 50MPa. Maintain the pressure at the final pressure for 10min to obtain a graphite bipolar plate.

[0070] Comparative Example 2

[0071] Weigh 10g of commercially available Toray carbon nanotubes with an average length of 20nm (10% of the mass of graphite) and 100g of 200-mesh microcrystalline graphite, place them on a vibration table for compaction treatment, with an amplitude of 100mm, a frequency of 400 times / min, and a vibration time of 5min. Place the compacted material in a molding cavity (sodium stearate is applied to the inside of the molding cavity as a release agent) and perform program pressure increase, with an initial pressure of 5MPa, a pressure increase rate of 2.5MPa / min, and a final pressure of 50MPa. Maintain the pressure at the final pressure for 15min to obtain a graphite bipolar plate.

[0072] Comparative Example 3

[0073] Weigh 10g of commercially available Toray carbon nanotubes with an average length of 50nm (10% of the mass of graphite), 50g of 200-mesh microcrystalline graphite and 50g of 150-mesh expanded graphite, and place them on a vibration table for compaction treatment, with an amplitude of 80mm, a frequency of 300 times / min, and a vibration time of 5min. The compacted materials are placed in a mold cavity (silicone oil is applied to the inside of the mold cavity as a release agent), and the program is increased. The initial pressure is 5MPa, the pressure increase rate is 2.5MPa / min, the final pressure is 50MPa, and the pressure is maintained at the final pressure for 20min to obtain a graphite bipolar plate.

[0074] Performance Testing

[0075] (1) Thickness test: Take six different locations in the flow channel area of ​​the bipolar plate, use a thickness gauge to test the thickness, and record and calculate the average value.

[0076] (2) Conductivity test: The conductivity of the composite board was measured using an RTS-9 dual-electricity four-probe measuring instrument. In order to eliminate the contact resistance between the metal probe and the sample, the DC four-probe method was used to directly test the conductivity.

[0077] (3) Bending strength test: The bending resistance of the composite board was measured using a WD-10D universal testing machine. The three-point bending method was used to test the bending strength of the composite board. The test steps are as follows:

[0078] ① Make the sample into a long strip with a width of 10mm.

[0079] ② Adjust the support span so that the pressure head and support head are perpendicular to the sample axis.

[0080] ③ The pressure head is 10mm / s 2 The load is applied uniformly and without impact until the sample breaks, and the breaking load value is read.

[0081] The flexural strength is calculated according to formula 1:

[0082] δ F =3PL / 2bh 2 Formula 1

[0083] In formula 1, δ F : flexural strength (MPa), P: breaking load value (N), L: support span (30mm), B: sample width (mm), h: sample thickness (mm).

[0084] Table 1 Performance test of graphite bipolar plates obtained in the examples and comparative examples

[0085] Bipolar plate thickness / mm Conductivity S / cm Bending strength / MPa Example 1 0.75 620 98 Example 2 0.83 601 75 Example 3 0.69 579 102 Comparative Example 1 1.53 356 65 Comparative Example 2 1.53 376 56 Comparative Example 3 1.53 402 62

[0086] Figure 1 This is a transmission electron microscope photo of the modified carbon nanotubes obtained in Example 1. Figure 2 is a transmission electron microscope photograph of the modified carbon nanotubes obtained in Example 3; Figure 1 and Figure 2 It can be seen that: when the temperature of the second pyrolysis is 600°C, carbon nanotubes begin to appear in the product, but their length is short, and in the TEM image, they are dot-like structures; when the temperature of the second pyrolysis rises to 1000°C, it can be clearly seen that the length of the carbon nanotubes is 20μm, which can be understood as the agglomeration and growth of the catalyst particles, which promotes the growth of the carbon nanotubes. Comparing Table 1, the difference between the modified carbon nanotubes after pyrolysis and the commercially available carbon nanotubes can be intuitively understood, and the thickness, conductivity and bending strength of the graphite bipolar plate are greatly improved; especially in Example 3, when the temperature of the second pyrolysis reaches 1000°C, the average length of the modified carbon nanotubes is 20μm, and the bending strength of the graphite bipolar plate after molding reaches 102MPa, which greatly improves the bending strength of the graphite bipolar plate; at the same time, the conductivity is also significantly improved.

[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A graphite bipolar plate, It is characterized in that The method is prepared from the following raw materials: graphite and modified carbon nanotubes; The mass of the modified carbon nanotubes is 1-10% of the mass of the graphite; The method for preparing the modified carbon nanotubes comprises the following steps: Mixing phenolic resin, a catalyst and an alcohol solvent, and sequentially curing and pyrolyzing them to obtain the modified carbon nanotubes; The catalyst is a metal salt; the metal salt includes metal nitrate or ferrocene; the metal nitrate includes one or more of ferric nitrate, nickel nitrate, manganese nitrate and cobalt nitrate; The curing comprises sequentially performing a first curing and a second curing; The first curing temperature is 70-80°C and the time is 8-12h; The second curing temperature is 100-120°C and the time is 20-24h; The pyrolysis comprises sequentially performing a first pyrolysis and a second pyrolysis; The temperature of the first pyrolysis is 300-500°C, the holding time is 20-30min, and the rate of heating to the first pyrolysis temperature is 5°C / min; The temperature of the second pyrolysis is 600-1200°C, the holding time is 30-60min, and the rate of increasing from the temperature of the first pyrolysis to the temperature of the second pyrolysis is 1°C / min; The pyrolysis is carried out under a protective atmosphere; The phenolic resin, the catalyst and the alcohol solvent are mixed comprising: dispersing the catalyst in the alcohol solvent, and then adding the phenolic resin and stirring and mixing; the stirring and mixing speed is 6000 ~ 10000rpm, time is 40min ~ 2h; The method for preparing the graphite bipolar plate comprises the following steps: Mixing graphite and modified carbon nanotubes, and performing tapping treatment and cold pressing in sequence to obtain the graphite bipolar plate; The pressure of the cold press molding is programmed pressure increase, and the parameters of the programmed pressure increase include: an initial pressure of 5MPa, a pressure increase rate of 2.5MPa / min, a terminal pressure of 50MPa, and a holding time of the terminal pressure of 10-20min.

2. The graphite bipolar plate according to claim 1, It is characterized in that The mass of the metal salt is 0.25-1% of the mass of the phenolic resin.

3. The graphite bipolar plate according to claim 1, It is characterized in that The alcohol solvent includes one or more of isopropyl alcohol, butanediol and isoprene diol.

4. The method for preparing the graphite bipolar plate according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Mixing graphite and modified carbon nanotubes, and performing tapping treatment and cold pressing in sequence to obtain the graphite bipolar plate; The pressure of the cold press molding is programmed pressure increase, and the parameters of the programmed pressure increase include: an initial pressure of 5MPa, a pressure increase rate of 2.5MPa / min, a terminal pressure of 50MPa, and a holding time of the terminal pressure of 10-20min.

5. The preparation method according to claim 4, It is characterized in that The parameters of the vibration treatment include: the vibration amplitude of the vibration table is 0.01-100 mm, the frequency is 1-400 times / min, and the vibration time is 3-5 min.