A high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance and preparation method thereof
Modification of silica wet gel and grafting of polyimide through chemical liquid phase modification method solves the structural problems of SiO2 aerogel in extreme temperature difference environments and achieves high thermal insulation, high transparency and UV shielding High-performance aerogel materials to meet the needs of the aerospace field.
Patent Information
- Application Number
- CN202211685237.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing SiO2 aerogels are prone to structural damage in extreme temperature difference environments, and their optical transmittance is lower than that of glass, resulting in energy loss and insufficient mechanical properties.
The chemical liquid phase modification method is used to modify the silica wet gel and graft polyimide to form a core-shell protection effect, maintain the original micromorphology and three-dimensional network structure of the SiO2 gel, and prepare a UV-shielding High performance transparent airgel insulation.
The airgel material has achieved high thermal insulation, high transparency, high and low temperature resistance and UV shielding properties, meeting the needs of aerospace and other fields, and reducing the negative impact of ultraviolet rays on material performance.
Smart Images

Figure CN115893429B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal insulation materials, and in particular relates to a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance and a preparation method thereof. Background Art
[0002] During deep space exploration, there is an extreme temperature difference of -200 to 200°C due to factors such as the temperature difference of the celestial body itself and the presence or absence of direct sunlight. The porthole, as an important observation window in the spacecraft, is exposed to space and is easily hit by space debris. Moreover, it is made of quartz glass, which is a heavy material, resulting in energy loss and large heat loss.
[0003] Aerogel is one of the solid materials with the lowest apparent density, with a porosity of 80-98%. Among them, SiO2 aerogel is one of the representatives of transparent aerogel, with simple synthesis process, low cost, rapid development, and is widely used in aerospace and other fields. However, the optical transmittance of SiO2 aerogel is still lower than that of glass, and it is fragile and hygroscopic, with poor mechanical properties, limited temperature resistance, and structural damage will occur in low temperature environments.
[0004] Therefore, there is an urgent need to develop a lightweight and transparent silica aerogel material with excellent mechanical properties, temperature resistance and low thermal conductivity. Summary of the invention
[0005] In view of one or more technical problems existing in the prior art, the present invention provides a high and low temperature resistant transparent aerogel thermal insulation material with UV shielding performance and a preparation method thereof. The preparation method provided by the present invention has a simple process and low cost. The prepared aerogel material has high thermal insulation, high transparency, high and low temperature resistance and UV shielding performance, and can meet different needs.
[0006] In a first aspect, the present invention provides a method for preparing a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance, the preparation method comprising the following steps:
[0007] S1. Adding a catalyst to an organosilicon solution, subjecting the solution to gelation and aging to obtain a wet gel; the organosilicon solution is obtained by dissolving an organosilicon compound in an alcohol;
[0008] S2. placing the wet gel in a silane coupling agent for modification, and then replacing the solvent to obtain a modified wet gel;
[0009] S3. placing the modified wet gel in a dianhydride solution, a diamine solution and an imidization agent in sequence for grafting modification to obtain the transparent aerogel thermal insulation material.
[0010] Preferably, in step S1, the gelation treatment is carried out by keeping the temperature at 30 to 60°C for 12 to 48 hours;
[0011] The aging treatment is aging in ethanol for 12 hours.
[0012] Preferably, the catalyst is an acid solution or an alkaline solution; preferably, the acid solution is at least one of hydrochloric acid and nitric acid; and the alkaline solution is at least one of ammonia water and sodium hydroxide solution;
[0013] The concentration of the acid solution and / or the alkaline solution is 0.15 to 0.75 mol / L.
[0014] Preferably, the organosilicon compound accounts for 15-45% of the total mass of the organosilicon compound, the alcohol substance and the water in the catalyst, preferably 45%;
[0015] The organosilicon compound is at least one of methyl orthosilicate and ethyl orthosilicate;
[0016] The alcohol substance is at least one of methanol, ethanol and isopropanol.
[0017] Preferably, in step S2, the modification treatment is carried out at 30-80°C for 12-48h.
[0018] Preferably, the silane coupling agent is at least one of KH-550, KH-560 and KH-570;
[0019] The solvent used in the solvent replacement is at least one of N-methylpyrrolidone, N,N'-dimethylacetamide and N,N'-dimethylformamide.
[0020] Preferably, in step S3, the modified wet gel is placed in a dianhydride solution, a diamine solution and an imidization agent in sequence at 30 to 80°C, and modified for 12 to 48 hours respectively to complete the graft modification.
[0021] Preferably, the dianhydride is at least one of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, hexafluoro dianhydride and pyromellitic dianhydride;
[0022] The diamine is at least one of 4,4'-diaminodiphenyl ether, 1,12-diaminododecane, and 2,2'-dimethylbenzidine; and / or
[0023] The imidization agent comprises pyridine and acetic anhydride.
[0024] Preferably, the amount of the dianhydride is 0.001 to 0.004 mol, preferably 0.001 mol;
[0025] The amount of the diamine substance is 0.001 to 0.004 mol, preferably 0.001 mol;
[0026] The amount of pyridine in the imidization agent is 0.001-0.004 mol, preferably 0.001 mol, and the amount of acetic anhydride is 0.001-0.004 mol, preferably 0.001 mol.
[0027] The present invention provides, in a second aspect, a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance, which is prepared by the preparation method described in the first aspect.
[0028] Compared with the prior art, the present invention has at least the following beneficial effects:
[0029] The present invention first prepares silicon dioxide wet gel, and then adopts a chemical liquid phase modification method to modify and graft polyimide on its surface to form a core-shell protection effect; in this way, the original microscopic morphology of the SiO2 gel can be maintained to the greatest extent, thereby maintaining the three-dimensional network structure characteristics of the SiO2 aerogel.
[0030] The preparation method of the present invention has simple process and low cost. The organic matter used for modification does not give the SiO2 aerogel material color characteristics, nor does it change its microscopic morphology. The obtained aerogel material has high thermal insulation, high transparency, high and low temperature resistance and UV shielding properties, which can meet the needs of transparent thermal insulation in aerospace and other fields, and can also be used in environments with ultraviolet radiation to reduce the negative impact of ultraviolet rays on the degradation of material performance, thereby realizing the diversification of aerogel application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 This is a physical picture of the high and low temperature resistant transparent aerogel thermal insulation material with UV shielding performance provided in Example 5 of the present invention;
[0033] Figure 2 This is a physical comparison diagram of the high and low temperature resistant transparent aerogel insulation material with ultraviolet shielding performance provided in Example 5 of the present invention before and after being treated with liquid nitrogen and 200° C.;
[0034] Figure 3is a transmittance curve of a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance provided in Example 5 of the present invention;
[0035] Figure 4 is an absorbance curve of a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance provided in Example 5 of the present invention;
[0036] Figure 5 This is an experimental diagram of the contact angle between the high and low temperature resistant transparent aerogel insulation material with UV shielding performance and water provided in Example 5 of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0038] In a first aspect, the present invention provides a method for preparing a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance, the preparation method comprising the following steps:
[0039] S1. Adding a catalyst to an organosilicon solution, subjecting the solution to gelation and aging to obtain a wet gel; the organosilicon solution is obtained by dissolving an organosilicon compound in an alcohol;
[0040] S2. placing the wet gel in a silane coupling agent for modification, and then replacing the solvent to obtain a modified wet gel;
[0041] S3. placing the modified wet gel in a dianhydride solution, a diamine solution and an imidizing agent in sequence for grafting modification to obtain the transparent aerogel thermal insulation material; the present invention places the modified wet gel in a dianhydride solution and a diamine solution in sequence for modification, grafting polyamic acid on the surface of the wet gel, and then imidizing under the action of an imidizing agent to graft polyimide on the surface of the wet gel.
[0042] The present invention first prepares silicon dioxide wet gel, and then adopts a chemical liquid phase modification method to modify and graft polyimide on its surface to form a core-shell protection effect; in this way, the original microscopic morphology of the SiO2 gel can be maintained to the greatest extent, thereby maintaining the three-dimensional network structure characteristics of the SiO2 aerogel.
[0043] The preparation method of the present invention has simple process and low cost. The organic matter used for modification does not impart color characteristics to the SiO2 aerogel material, nor does it change its microscopic morphology. The obtained composite aerogel has high thermal insulation, high transparency, high and low temperature resistance and UV shielding properties, which can meet the needs of transparent thermal insulation in aerospace and other fields, and can also be used in environments with ultraviolet radiation to reduce the negative impact of ultraviolet rays on the degradation of material performance, thereby realizing the diversification of aerogel application fields.
[0044] According to some preferred embodiments, in step S1, the gelation treatment is to keep warm at 30-60°C (for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C) for 12-48h (for example, 12h, 15h, 20h, 24h, 25h, 30h, 36h, 40h, 45h or 48h);
[0045] The aging treatment is aging in ethanol for 12 hours.
[0046] According to some preferred embodiments, the catalyst is an acid solution or an alkaline solution; preferably, the acid solution is at least one of hydrochloric acid and nitric acid; the alkaline solution is at least one of ammonia water and sodium hydroxide solution;
[0047] The concentration of the acid solution and / or the alkaline solution is 0.15 to 0.75 mol / L (for example, 0.15 mol / L, 0.30 mol / L, 0.45 mol / L, 0.60 mol / L or 0.75 mol / L). The concentration of the acid solution or alkaline solution of the present invention will affect the gelation speed. The higher the concentration, the faster the gelation speed. If the concentration is too high, the gelation speed is too fast, which is not conducive to transferring the wet gel to the mold.
[0048] According to some preferred embodiments, the organosilicon compound accounts for 15 to 45% (for example, 15%, 20%, 25%, 30%, 35%, 40%, or 45%) of the total mass of the organosilicon compound, the alcohol substance and the water in the catalyst, preferably 45%; different mass fractions of the organosilicon compound of the present invention will affect the shrinkage rate of the aerogel, and the smaller the mass fraction of the organosilicon compound, the greater the shrinkage rate.
[0049] The organosilicon compound is at least one of methyl orthosilicate and ethyl orthosilicate. The present invention selects an organosilicon compound with a small molecular volume as a silicon source, which can effectively reduce the microstructure size of the aerogel material and avoid reducing its optical transmittance due to excessive microstructure.
[0050] The alcohol substance is at least one of methanol, ethanol and isopropanol.
[0051] According to some preferred embodiments, in step S2, the modification treatment is carried out at 30-80°C (for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C) for 12-48h (for example, 12h, 15h, 20h, 24h, 25h, 30h, 36h, 40h, 45h or 48h).
[0052] According to some preferred embodiments, the silane coupling agent is at least one of KH-550, KH-560 and KH-570;
[0053] The solvent used in the solvent replacement is at least one of N-methylpyrrolidone, N,N'-dimethylacetamide and N,N'-dimethylformamide;
[0054] The invention places the prepared SiO2 wet gel in a silane coupling agent, modifies the surface of the SiO2 wet gel, and then replaces the gel with a solvent to obtain the modified wet gel.
[0055] According to some preferred embodiments, in step S3, at 30-80°C (for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C), the modified wet gel is sequentially placed in a dianhydride solution, a diamine solution and an imidization agent, and modified for 12-48h (for example, 12h, 15h, 20h, 24h, 25h, 30h, 36h, 40h, 45h or 48h) to complete the grafting modification. It should be noted that after the grafting modification, the steps of solvent replacement and drying are also included; wherein, ethanol is used for solvent replacement, and supercritical CO2 drying is used for drying.
[0056] It should be noted that the dianhydride solution of the present invention is obtained by dissolving dianhydride in an organic solvent; the diamine solution is obtained by dissolving diamine in an organic solvent; and the imidization reagent is obtained by dissolving pyridine and acetic anhydride in an organic solvent; wherein the organic solvent is at least one of N-methylpyrrolidone, N,N'-dimethylacetamide and N,N'-dimethylformamide.
[0057] The invention first places the modified wet gel in a dianhydride solution, grafts the dianhydride on the surface of the wet gel, then places it in a diamine solution, grafts polyamic acid on the surface of the wet gel through the reaction of the dianhydride and the diamine, and then performs imidization under the action of an imidization agent, grafts polyimide on the surface of the wet gel, and completes the grafting modification of the wet gel surface.
[0058] According to some preferred embodiments, the dianhydride is at least one of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, hexafluoro dianhydride and pyromellitic dianhydride;
[0059] The diamine is at least one of 4,4'-diaminodiphenyl ether, 1,12-diaminododecane, and 2,2'-dimethylbenzidine; and / or
[0060] The imidization agent comprises pyridine and acetic anhydride; the imidization agent of the present invention mainly plays the role of promoting the imidization of polyamic acid to form polyimide.
[0061] According to some preferred embodiments, the amount of the dianhydride is 0.001 to 0.004 mol (for example, 0.001 mol, 0.002 mol, 0.003 mol or 0.004 mol), preferably 0.001 mol;
[0062] The amount of the diamine substance is 0.001 to 0.004 mol (for example, 0.001 mol, 0.002 mol, 0.003 mol or 0.004 mol), preferably 0.001 mol;
[0063] The amount of pyridine in the imidization reagent is 0.001-0.004 mol (for example, 0.001 mol, 0.002 mol, 0.003 mol or 0.004 mol), preferably 0.001 mol, and the amount of acetic anhydride is 0.001-0.004 mol (for example, 0.001 mol, 0.002 mol, 0.003 mol or 0.004 mol), preferably 0.001 mol.
[0064] The increase in the molar amount of dianhydride, diamine, pyridine and acetic anhydride in the present invention is beneficial to improving the reinforcing effect, but too high a molar amount will cause the gel to crack and destroy the three-dimensional network structure.
[0065] The present invention provides, in a second aspect, a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance, which is prepared by the preparation method described in the first aspect.
[0066] The aerogel composite material prepared by the invention has a transparent appearance, a transmittance of 80 to 90% at a wavelength of 800 nm, and a certain ultraviolet shielding performance; a thermal conductivity of 0.02375 to 0.02726 W / (mK), and has excellent heat insulation performance; after being treated at low temperature (liquid nitrogen) and high temperature (200°C), the shape remains unchanged, and has excellent high and low temperature resistance; meanwhile, the contact angle is about 106°, and has excellent hydrophobic performance.
[0067] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with embodiments.
[0068] The materials and reagents in the present invention can be directly purchased on the market or synthesized by themselves, and there is no limitation on the specific models.
[0069] Example 1
[0070] S1. Add 0.15 mol / L hydrochloric acid to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 30°C for 24 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a silicon dioxide wet gel; wherein the organosilicon solution is obtained by mixing methyl orthosilicate and methanol; and methyl orthosilicate accounts for 15% of the total mass of water in methyl orthosilicate, methanol and hydrochloric acid; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0071] S2. The silica wet gel was placed in a KH-550 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N-methylpyrrolidone for 12 hours to obtain a modified wet gel;
[0072] S3. At 30°C, the modified wet gel is placed in 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride solution, 4,4'-diaminodiphenyl ether solution, and imidization reagent in turn, and modified for 12 hours respectively, to complete the polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, the 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride solution is obtained by dissolving 0.001 mol 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride in 40 mL N-methylpyrrolidone; the 4,4'-diaminodiphenyl ether solution is obtained by dissolving 0.001 mol 4,4'-diaminodiphenyl ether in 40 mL N-methylpyrrolidone; the imidization reagent is obtained by dissolving 0.001 mol acetic anhydride and 0.001 mol pyridine in 40 mL N-methylpyrrolidone.
[0073] The aerogel material prepared in Example 1 has a transmittance of 82.09% at a wavelength of 800 nm.
[0074] Example 2
[0075] S1. Add 0.30 mol / L ammonia water to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 60°C for 24 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a silicon dioxide wet gel; wherein the organosilicon solution is obtained by mixing tetraethyl orthosilicate and ethanol, and tetraethyl orthosilicate accounts for 25% of the total mass of water in tetraethyl orthosilicate, ethanol and ammonia water; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0076] S2. The silica wet gel was placed in a KH-550 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N,N'-dimethylacetamide for 12 hours to obtain a modified wet gel;
[0077] S3. At 60°C, the modified wet gel is placed in 3,3',4,4'-biphenyltetracarboxylic acid dianhydride solution, 1,12-diaminododecane solution, and imidization reagent in turn, and modified for 12 hours respectively, to complete polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride solution is obtained by dissolving 0.001 mol 3,3',4,4'-biphenyltetracarboxylic acid dianhydride in 40 mL N,N'-dimethylacetamide; 1,12-diaminododecane is obtained by dissolving 0.001 mol 1,12-diaminododecane in 40 mL N,N'-dimethylacetamide; and the imidization reagent is obtained by dissolving 0.001 mol acetic anhydride and 0.001 mol pyridine in 40 mL N,N'-dimethylacetamide.
[0078] The aerogel material prepared in Example 2 has a transmittance of 83.14% at a wavelength of 800 nm.
[0079] Example 3
[0080] S1. Add 0.45 mol / L hydrochloric acid to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 80°C for 24 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a wet silica gel; wherein the organosilicon solution is obtained by mixing methyl orthosilicate and methanol, and methyl orthosilicate accounts for 35% of the total mass of water in methyl orthosilicate, methanol and hydrochloric acid; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0081] S2. The silica wet gel was placed in a KH-560 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N,N'-dimethylformamide for 12 hours to obtain a modified wet gel;
[0082] S3. At 80°C, the modified wet gel is placed in a hexafluorodianhydride solution, a 2,2'-dimethylbenzidine solution, and an imidization agent in turn, and modified for 12 hours respectively, to complete the polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, the hexafluorodianhydride solution is obtained by dissolving 0.001 mol of hexafluorodianhydride in 40 mL of N,N'-dimethylformamide; the 2,2'-dimethylbenzidine solution is obtained by dissolving 0.001 mol of 2,2'-dimethylbenzidine in 40 mL of N,N'-dimethylformamide; the imidization agent is obtained by dissolving 0.001 mol of acetic anhydride and 0.001 mol of pyridine in 40 mL of N,N'-dimethylformamide.
[0083] The aerogel material prepared in Example 3 has a transmittance of 84.06% at a wavelength of 800 nm.
[0084] Example 4
[0085] S1. Add 0.60 mol / L ammonia water to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 60°C for 24 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a silicon dioxide wet gel; wherein the organosilicon solution is obtained by mixing tetraethyl orthosilicate and ethanol, and tetraethyl orthosilicate accounts for 45% of the total mass of water in tetraethyl orthosilicate, ethanol and ammonia water; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0086] S2. The silica wet gel was placed in KH-570 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N-methylpyrrolidone for 12 hours to obtain a modified wet gel;
[0087] S3. At 60°C, the modified wet gel is placed in a solution of pyromellitic anhydride, a solution of 2,2'-dimethylbenzidine, and an imidizing agent in turn, and modified for 12 hours respectively, to complete the polyimide grafting modification on the surface of the gel, and finally washed with ethanol and the solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, the pyromellitic anhydride solution is obtained by dissolving 0.001 mol of pyromellitic anhydride in 40 mL of N-methylpyrrolidone; the 2,2'-dimethylbenzidine solution is obtained by dissolving 0.001 mol of 2,2'-dimethylbenzidine in 40 mL of N-methylpyrrolidone; the imidizing agent is obtained by dissolving 0.001 mol of acetic anhydride and 0.001 mol of pyridine in 40 mL of N-methylpyrrolidone.
[0088] The aerogel material prepared in Example 4 has a transmittance of 85.24% at a wavelength of 800 nm.
[0089] Example 5
[0090] S1. Add 0.75 mol / L ammonia water to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 30°C for 24 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a silicon dioxide wet gel; wherein the organosilicon solution is obtained by mixing methyl orthosilicate and methanol, and methyl orthosilicate accounts for 45% of the total mass of water in methyl orthosilicate, methanol and ammonia water; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0091] S2. The silica wet gel was placed in a KH-550 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N,N'-dimethylacetamide for 12 hours to obtain a modified wet gel;
[0092] S3. At 30°C, the modified wet gel is placed in a hexafluorodianhydride solution, a 1,12-diaminododecane solution, and an imidizing agent in turn, and modified for 12 hours respectively, to complete the polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, the hexafluorodianhydride solution is obtained by dissolving 0.001 mol of hexafluorodianhydride in 40 mL of N,N'-dimethylacetamide; the 1,12-diaminododecane solution is obtained by dissolving 0.001 mol of 1,12-diaminododecane in 40 mL of N,N'-dimethylacetamide; the imidizing agent is obtained by dissolving 0.001 mol of acetic anhydride and 0.001 mol of pyridine in 40 mL of N,N'-dimethylacetamide.
[0093] The aerogel material prepared in Example 5 has a transmittance of 88.98% at a wavelength of 800 nm. Figure 2 It can be seen that the aerogel material prepared in Example 5 is transparent, and its morphology remains unchanged before and after being treated with liquid nitrogen and 200°C, and it has excellent temperature resistance. Figure 4 It can be seen that the aerogel material prepared in Example 5 has excellent ultraviolet shielding performance; Figure 5 It can be seen that the contact angle between the aerogel material prepared in Example 5 and water is 105.1°, which has excellent hydrophobic properties.
[0094] Example 6
[0095] S1. Add 0.75 mol / L ammonia water to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 30°C for 12 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a silicon dioxide wet gel; wherein the organosilicon solution is obtained by mixing methyl orthosilicate and methanol, and methyl orthosilicate accounts for 45% of the total mass of water in methyl orthosilicate, methanol and ammonia water; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0096] S2. The silica wet gel was placed in a KH-550 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N,N'-dimethylacetamide for 12 hours to obtain a modified wet gel;
[0097] S3. At 30°C, the modified wet gel was placed in a hexafluorodianhydride solution, a 1,12-diaminododecane solution, and an imidizing agent in turn, and modified for 12 hours respectively, to complete the polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, the hexafluorodianhydride solution was obtained by dissolving 0.002 mol of hexafluorodianhydride in 40 mL of N,N'-dimethylacetamide; the 1,12-diaminododecane solution was obtained by dissolving 0.002 mol of 1,12-diaminododecane in 40 mL of N,N'-dimethylacetamide; and the imidizing agent was obtained by dissolving 0.002 mol of acetic anhydride and 0.002 mol of pyridine in 40 mL of N,N'-dimethylacetamide.
[0098] The aerogel material prepared in Example 6 has a transmittance of 88.02% at a wavelength of 800 nm, and its morphology remains unchanged before and after being treated with liquid nitrogen and 200° C., showing excellent temperature resistance.
[0099] Example 7
[0100] S1. Add 0.75 mol / L ammonia water to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 30°C for 24 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a silicon dioxide wet gel; wherein the organosilicon solution is obtained by mixing methyl orthosilicate and methanol, and methyl orthosilicate accounts for 45% of the total mass of water in methyl orthosilicate, methanol and ammonia water; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0101] S2. The silica wet gel was placed in a KH-550 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N,N'-dimethylacetamide for 12 hours to obtain a modified wet gel;
[0102] S3. At 30°C, the modified wet gel is placed in a hexafluorodianhydride solution, a 1,12-diaminododecane solution, and an imidizing agent in turn, and modified for 24 hours respectively, to complete the polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, the hexafluorodianhydride solution is obtained by dissolving 0.003 mol of hexafluorodianhydride in 40 mL of N,N'-dimethylacetamide; the 1,12-diaminododecane solution is obtained by dissolving 0.003 mol of 1,12-diaminododecane in 40 mL of N,N'-dimethylacetamide; the imidizing agent is obtained by dissolving 0.003 mol of acetic anhydride and 0.003 mol of pyridine in 40 mL of N,N'-dimethylacetamide.
[0103] The aerogel material prepared in Example 7 has a transmittance of 87.28% at a wavelength of 800 nm, and can maintain its morphology without significant change before and after being treated with liquid nitrogen and 200° C., and has excellent temperature resistance.
[0104] Example 8
[0105] S1. Add 0.75 mol / L ammonia water to the organosilicon solution, continue to stir on a magnetic stirrer until uniform, then transfer to a mold, place in an oven at 30°C for 24 hours, and then place in ethanol at room temperature for further aging for 12 hours to obtain a silicon dioxide wet gel; wherein the organosilicon solution is obtained by mixing methyl orthosilicate and methanol, and methyl orthosilicate accounts for 45% of the total mass of water in methyl orthosilicate, methanol and ammonia water; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm respectively;
[0106] S2. The silica wet gel was placed in a KH-550 silane coupling agent for modification for 12 hours, and then the solvent was replaced by soaking in N,N'-dimethylacetamide for 12 hours to obtain a modified wet gel;
[0107] S3. At 30°C, the modified wet gel is placed in a hexafluorodianhydride solution, a 1,12-diaminododecane solution, and an imidizing agent in turn, and modified for 48 hours respectively, to complete the polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein, the hexafluorodianhydride solution is obtained by dissolving 0.004 mol of hexafluorodianhydride in 40 mL of N,N'-dimethylacetamide; the 1,12-diaminododecane solution is obtained by dissolving 0.004 mol of 1,12-diaminododecane in 40 mL of N,N'-dimethylacetamide; the imidizing agent is obtained by dissolving 0.004 mol of acetic anhydride and 0.004 mol of pyridine in 40 mL of N,N'-dimethylacetamide.
[0108] The aerogel material prepared in Example 8 has a transmittance of 86.32% at a wavelength of 800 nm, and can maintain its morphology without significant change before and after being treated with liquid nitrogen and 200° C., and has excellent temperature resistance.
[0109] Comparative Example 1
[0110] Comparative Example 1 is basically the same as Example 5, except that: S1. 0.75 mol / L of ammonia water is added to the organosilicon solution, and the mixture is stirred on a magnetic stirrer until uniform, then transferred to a mold, allowed to stand in an oven at 30°C for 24 hours, and then placed in ethanol at room temperature for further aging for 12 hours to obtain a wet silica gel; wherein the organosilicon solution is obtained by mixing methyl orthosilicate and methanol, and methyl orthosilicate accounts for 5% of the total mass of water in methyl orthosilicate, methanol and ammonia water; the mold is a rectangular mold with a length, width and height of 80 mm, 80 mm and 40 mm, respectively.
[0111] The content of methyl orthosilicate is too low, resulting in severe shrinkage during the drying process, and the transparency of the obtained aerogel material is low.
[0112] Comparative Example 2
[0113] Comparative Example 2 is basically the same as Example 1, except that: S3. At 30°C, the modified wet gel is placed in a hexafluorodianhydride solution, a 1,12-diaminododecane solution, and an imidizing agent in turn, and modified for 12 hours respectively, to complete polyimide grafting modification on the gel surface, and finally washed with ethanol and solvent replaced, and dried with supercritical CO2 to obtain a transparent aerogel insulation material; wherein the hexafluorodianhydride solution is obtained by dissolving 0.006 mol of hexafluorodianhydride in 40 mL of N,N'-dimethylacetamide; the 1,12-diaminododecane solution is obtained by dissolving 0.006 mol of 1,12-diaminododecane in 40 mL of N,N'-dimethylacetamide; the imidizing agent is obtained by dissolving 0.006 mol of acetic anhydride and 0.006 mol of pyridine in 40 mL of N,N'-dimethylacetamide.
[0114] In Comparative Example 2, since the molar amounts of dianhydride, diamine, acetic anhydride and pyridine in the grafting modification process are too high, the gel is broken during the modification process and an aerogel with a complete structure cannot be formed.
[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a high and low temperature resistant transparent aerogel thermal insulation material with ultraviolet shielding performance, characterized in that: The preparation method comprises the following steps: S1. Adding a catalyst to an organosilicon solution, subjecting it to gelation treatment and aging treatment to obtain a wet gel; the organosilicon solution is obtained by dissolving an organosilicon compound in an alcohol substance; the organosilicon compound accounts for 15 to 45% of the total mass of the water in the organosilicon compound, the alcohol substance and the catalyst; the organosilicon compound is at least one of methyl orthosilicate and ethyl orthosilicate; S2. placing the wet gel in a silane coupling agent for modification, and then replacing the solvent to obtain a modified wet gel; S3. placing the modified wet gel in a dianhydride solution, a diamine solution and an imidization agent in sequence for grafting modification to obtain the transparent aerogel thermal insulation material.
2. The preparation method according to claim 1, characterized in that: In step S1, the gelation treatment is carried out by keeping the temperature at 30 to 60°C for 12 to 48 hours; The aging treatment is aging in ethanol for 12 hours.
3. The preparation method according to claim 1, characterized in that: The catalyst is an acid solution or an alkaline solution; The concentration of the acid solution and / or the alkaline solution is 0.15 to 0.75 mol / L.
4. The preparation method according to claim 3, characterized in that: The acid solution is at least one of hydrochloric acid and nitric acid; the alkaline solution is at least one of ammonia water and sodium hydroxide solution.
5. The preparation method according to claim 1, characterized in that: The alcohol substance is at least one of methanol, ethanol and isopropanol.
6. The preparation method according to claim 1, characterized in that: In step S2, the modification treatment is carried out at 30-80°C for 12-48h.
7. The preparation method according to claim 1, characterized in that: The silane coupling agent is at least one of KH-550, KH-560 and KH-570; The solvent used in the solvent replacement is at least one of N-methylpyrrolidone, N,N'-dimethylacetamide and N,N'-dimethylformamide.
8. The preparation method according to claim 1, characterized in that: In step S3, the modified wet gel is placed in a dianhydride solution, a diamine solution and an imidization agent in sequence at 30 to 80° C. and modified for 12 to 48 hours respectively to complete the graft modification.
9. The preparation method according to claim 8, characterized in that: The dianhydride is at least one of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, hexafluoro dianhydride and pyromellitic dianhydride; The diamine is at least one of 4,4'-diaminodiphenyl ether, 1,12-diaminododecane, and 2,2'-dimethylbenzidine; and / or The imidization agent comprises pyridine and acetic anhydride.
10. The preparation method according to claim 8, characterized in that: The amount of the dianhydride is 0.001 to 0.004 mol; The amount of the diamine substance is 0.001 to 0.004 mol; In the imidization reagent, the amount of pyridine is 0.001 to 0.004 mol, and the amount of acetic anhydride is 0.001 to 0.004 mol.
11. The preparation method according to claim 10, characterized in that: The amount of substance of the dianhydride is 0.001 mol; The amount of the diamine substance is 0.001 mol; In the imidization reagent, the amount of pyridine is 0.001 mol, and the amount of acetic anhydride is 0.001 mol.
12. A high and low temperature resistant transparent aerogel thermal insulation material with UV shielding performance, characterized in that: The preparation method is described in any one of claims 1 to 11.
Citation Information
Patent Citations
Polyimide-organosiloxane composite aerogel material and preparation method thereof
CN109593228A
Cited By
Preparation method of ultra-transparent aerogel sheet material
CN119612524A
A method for preparing a super-transparent aerogel sheet
CN119612524B
Preparation method and application of super-transparent silicon dioxide aerogel thermal insulation material