(C3H8N6I6)·3H2O compound, birefringent crystal and preparation method and use thereof
By dissolving melamine in aqueous hydroiodic acid solution and adding iodine, (C3H8N6I6)·3H2O birefringent crystals are prepared, which solves the problems of difficult preparation of existing birefringent crystal materials and insufficient birefringent index, and realizes high-performance birefringent crystals Prepare and apply to polarization devices.
Patent Information
- Application Number
- CN202211535727.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-02
AI Technical Summary
The existing birefringent crystal materials have problems such as difficult preparation, small size, large hardness, and too small birefringence, which are difficult to meet high-quality needs.
Using (C3H8N6I6)·3H2O compound, by dissolving melamine in aqueous hydroiodic acid and adding elemental iodine, heating and slowly cooling under constant magnetic force, a (C3H8N6I6)·3H2O birefringent crystal with super-large birefringent properties was formed.
The preparation of (C3H8N6I6)·3H2O birefringent crystals with short growth cycle and low cost is realized, and is used to prepare high-performance polarization devices, suitable for polarization beam splitting prisms, phase delay devices, etc. in the optical and communication fields.
Smart Images

Figure CN115894392B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a (C3H8N6I6)·3H2O compound, a birefringent crystal and a preparation method and application thereof. Technical Background
[0002] Double refraction is the phenomenon that when a light beam is incident on a crystal, it is decomposed into two beams that are refracted in different directions. They are linearly polarized lights with vibration directions perpendicular to each other. The fundamental reason for this phenomenon is the anisotropy of the crystal material. When light propagates in a heterogeneous body or a homogeneous body, two beams of refracted light can be observed. This phenomenon is called double refraction of light. One of the two refracted light beams always obeys the refractive index law. This refracted light beam is called ordinary light, or o light for short. The other refracted light beam does not obey the ordinary refractive index law. This light beam is called extraordinary light, or e light for short. Corresponding to n o (normal refractive index) and n e (Special refractive index). Birefringence is Δn=|n o -n e |. For a positive uniaxial crystal, n e >n o ; For negative uniaxial crystals, n e <n o .
[0003] Since birefringent crystals have the ability to modulate and polarize light, they can be used as polarization devices in linear optical devices, fiber optic sensors, and advanced optical communication systems. Currently, commercial birefringent crystals, such as MgF2, α-BaB2O4, CaCO3, YVO4, TiO2, and LiNbO3, still have various defects. Taking TiO2 as an example, it mainly exists in natural form, it is difficult to synthesize artificially, and it is small in size and hard. It is difficult to process. MgF2 birefringent crystal is a good crystal material for deep ultraviolet, but its birefringence is too small to be used for the manufacture of Glan prisms. It can only be used for Rochon prisms, and the light separation angle is small, the size is large, and it is inconvenient to use. With the development of society, human beings have more and more demand for birefringent crystals, and the quality requirements are getting higher and higher. Therefore, the discovery of new excellent birefringent optical crystal materials is still a problem to be solved. Summary of the invention
[0004] The object of the present invention is to provide a (C3H8N6I6)·3H2O compound, a birefringent crystal, and a preparation method and use thereof. The (C3H8N6I6)·3H2O crystal of the present invention has a large birefringent property, a short growth cycle, and low cost, and can be used to prepare a polarization device.
[0005] The technical solution of the present invention is as follows:
[0006] 1. A compound of (C3H8N6I6)·3H2O, wherein the chemical formula of the compound is (C3H8N6I6)·3H2O.
[0007] 2. (C3H8N6I6)·3H2O birefringent crystal, the (C3H8N6I6)·3H2O birefringent crystal belongs to the monoclinic system and the P121 / n space group.
[0008] The unit cell parameters of the (C3H8N6I6)·3H2O birefringent crystal are Z=4.
[0009] The (C3H8N6I6)·3H2O crystal structure is composed of melamine organic cation (C3H8N6) 2+ 、Inorganic iodine chain anion (I3) - and water molecules. Among them (C3H8N6) 2+ The cations are connected to each other by hydrogen bonds with water molecules, forming one-dimensional infinite chains parallel to each other. In addition, (I3) - Anions are interspersed between chains, forming an alternating three-dimensional "intercalation" structure.
[0010] 3. A method for preparing a (C3H8N6I6)·3H2O birefringent crystal comprises the following steps performed in sequence:
[0011] a. Dissolve melamine (C3H8N6) in a 47% by mass aqueous solution of hydroiodic acid, and heat to 50-60°C under constant magnetic stirring to obtain a clear solution, wherein the molar ratio of C3H8N6 to HI is 1:1-10;
[0012] b. Then add elemental iodine, and continue stirring at 50-60°C until the solution is clear, wherein the molar ratio of C3H8N6 to I2 is 1:1-2;
[0013] c. Finally, the temperature was cooled to room temperature at a rate of 1°C / day to obtain the (C3H8N6I6)·3H2O birefringent crystal.
[0014] 4. Use of the (C3H8N6I6)·3H2O birefringent crystal. The (C3H8N3I6)·3H2O birefringent crystal is used to prepare polarization devices.
[0015] 5. A polarizing device, prepared from the (C3H8N3I6)·3H2O birefringent crystal.
[0016] The polarization device is an optical polarizer, a beam displacer, a circulator, an optical isolator or an optical modulator.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The present invention provides a new birefringent crystal, wherein the (C3H8N6I6)·3H2O birefringent crystal has an extremely large birefringence, which is much higher than that of most reported birefringent crystals;
[0019] (2) The reagents and raw materials used in the method of the present invention have low toxicity to the human body, short growth cycle and low cost;
[0020] (3) The (C3H8N6I6)·3H2O birefringent crystal can be used to make polarization devices;
[0021] (4) The polarization device made of the birefringent crystal of the present invention has important applications in the fields of optics and communications, and can be used to make polarization beam splitting prisms, phase delay devices, electro-optical modulation devices, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the working principle diagram of an optical isolator made of (C3H8N6I6)·3H2O crystal, where ①⑤ are couplers, ②④ are birefringent crystals, and ③ is an optically active material.
[0023] Figure 2 It is the X-ray diffraction pattern of the (C3H8N6I6)·3H2O polycrystalline powder of the present invention and the X-ray diffraction pattern based on the (C3H8N6I6)·3H2O crystal structure simulation.
[0024] Figure 3 This is the crystal structure diagram of (C3H8N6I6)·3H2O of the present invention.
[0025] Figure 4 This is the transmission spectrum of (C3H8N6I6)·3H2O crystal.
[0026] Figure 5 This is a photo of the single crystal obtained in Example 1.
[0027] Figure 6 The refractive index and birefringence of (C3H8N6I6)·3H2O at different wavelengths were theoretically calculated. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the embodiments and drawings. Those skilled in the art will appreciate that the following embodiments are not intended to limit the scope of protection of the present invention, and any improvements and changes made on the basis of the present invention are within the scope of protection of the present invention.
[0029] Examples 1-5 are about the preparation method of (C3H8N6I6)·3H2O birefringent crystal.
[0030] Example 1
[0031] The method for preparing a (C3H8N6I6)·3H2O birefringent crystal comprises the following steps performed in sequence:
[0032] C3H6N6 (5.0 g) was dissolved in a 47% HI aqueous solution (25 mL) and heated to 50°C under constant magnetic stirring to obtain a clear solution. Subsequently, iodine (10 g) was added to the hot solution. Then, the reaction mixture was heated at 50°C and stirred thoroughly until dissolved. Finally, large-sized crystals were slowly grown at a rate of 1°C / day by a slow cooling method, and block crystals were separated by filtration with filter paper to obtain (C3H8N6I6)·3H2O.
[0033] like Figure 2 As shown, the powder X-ray diffraction pattern obtained from the experiment is consistent with the pattern obtained by fitting based on its single crystal structure.
[0034] Example 2
[0035] The method for preparing a (C3H8N6I6)·3H2O birefringent crystal comprises the following steps performed in sequence:
[0036] First, C3H6N6 (5.0 g) was dissolved in a 47% HI aqueous solution (20 mL) and heated to 50°C under mechanical stirring to obtain a clear solution. Subsequently, iodine (10 g) was added to the hot solution. Then, the reaction mixture was heated at 50°C and stirred until dissolved. Finally, a slow cooling method was used to slowly grow large-sized crystals at a rate of 1°C / day, and the block crystals were separated by filtration with filter paper to obtain (C3H8N3I6)·3H2O.
[0037] The powder X-ray diffraction pattern obtained in the experiment of this example is consistent with the pattern obtained by fitting based on its single crystal structure.
[0038] Example 3
[0039] The method for preparing a (C3H8N6I6)·3H2O birefringent crystal comprises the following steps performed in sequence:
[0040] First, C3H6N6 (5.0 g) was dissolved in a 47% HI aqueous solution (20 mL), heated to 50°C under mechanical stirring, and 5 mL of distilled water was added to obtain a clear solution. Subsequently, iodine (10 g) was added to the hot solution. Then, the reaction mixture was heated at 50°C and stirred until dissolved. Finally, a slow cooling method was used to slowly grow large-sized crystals at a rate of 1°C / day to obtain (C3H8N6I6)·3H2O.
[0041] The powder X-ray diffraction pattern obtained in the experiment of this example is consistent with the pattern obtained by fitting based on its single crystal structure.
[0042] Example 4
[0043] The method for preparing a (C3H8N6I6)·3H2O birefringent crystal comprises the following steps performed in sequence:
[0044] First, C3H6N6 (5.0 g) was dissolved in a 47% HI aqueous solution (15 mL), heated to 50°C under mechanical stirring, and 10 mL of distilled water was added to obtain a clear solution. Subsequently, iodine (20 g) was added to the hot solution. Then, the reaction mixture was heated at 50°C and stirred until dissolved. Finally, a slow cooling method was used to slowly grow large-sized crystals at a rate of 1°C / day to obtain (C3H8N6I6)·3H2O.
[0045] The powder X-ray diffraction pattern obtained in the experiment of this example is consistent with the pattern obtained by fitting based on its single crystal structure.
[0046] Example 5
[0047] The method for preparing a (C3H8N6I6)·3H2O birefringent crystal comprises the following steps performed in sequence:
[0048] First, C3H6N6 (5.0 g) was dissolved in a 47% HI aqueous solution (30 mL) and heated to 55°C under mechanical stirring to obtain a clear solution. Subsequently, iodine (10 g) was added to the hot solution. Then, the reaction mixture was heated at 55°C and stirred until dissolved. Finally, a slow cooling method was used to slowly grow large-sized crystals at a rate of 1.5°C / day to obtain (C3H8N6I6)·3H2O.
[0049] The powder X-ray diffraction pattern obtained in the experiment of this example is consistent with the pattern obtained by fitting based on its single crystal structure.
[0050] The (C3H8N6I6)·3H2O birefringent crystal obtained in Example 1 was tested for transmission spectrum. Figure 4 As shown, from Figure 4 It can be seen that the transmission cutoff edge of the crystal is 671 nm.
[0051] The transmission cutoff edge of the crystal is 671nm; the crystal is not easy to break and does not absorb moisture. First-principle calculations of the optical properties of (C3H8N6I6)·3H2O revealed that its birefringence is as high as 1.7 in the infrared region and as high as 2.8 in the visible region (e.g. Figure 6 It is the largest birefringent crystal reported so far.
[0052] The above specific implementation methods are only detailed explanations of the technical solutions of the present invention. The present invention is not limited to the above embodiments. Those skilled in the art should understand that any improvements and substitutions based on the above principles and spirits on the basis of the present invention should be within the protection scope of the present invention.
Claims
1. (C3H8N6I6)·3H2O birefringent crystal, characterized by: The (C3H8N6I6)·3H2O birefringent crystal belongs to the monoclinic system. P 121 / n Space group; the unit cell parameters of the (C3H8N6I6)·3H2O birefringent crystal are a =9.4872(1)Å, b =27.2664(3) Å, c =14.9897(2) Å, V =3840.71(9) Å 3 , Z =4.
2. The method for preparing the (C3H8N6I6)·3H2O birefringent crystal according to claim 1, characterized in that: The steps include the following steps in order: a. Dissolve melamine in an aqueous solution containing hydroiodic acid, and heat to 50-60°C under constant magnetic stirring to obtain a clear solution in which the molar ratio of melamine to HI is 1:1-10; b. Then add elemental iodine, and continue stirring at 50-60°C until the solution is clear, wherein the molar ratio of melamine to I2 is 1:1-2; c. Finally, the temperature is lowered to room temperature at a rate of 1 °C / day to obtain the (C3H8N6I6) ·3H2O birefringent crystal.
3. Use of the (C3H8N6I6)·3H2O birefringent crystal according to claim 1, characterized in that: The (C3H8N6I6)·3H2O birefringent crystal is used for preparing polarization devices.
4. A polarization device, characterized in that: The invention is prepared from the (C3H8N6I6)·3H2O birefringent crystal as claimed in claim 1.
5. The polarization device according to claim 4, characterized in that: The polarization device is an optical polarizer, a beam displacer, a circulator, an optical isolator or an optical modulator.