Gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing and preparation method thereof
Through the gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing, the photothermal properties of perfluorodecalin nanoparticles and antimicrobial peptides are used to solve the dual problems of wound hypoxia and antibacterial resistance, and achieve efficient wound healing. Healing and antibacterial effects.
Patent Information
- Application Number
- CN202211444334.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-18
AI Technical Summary
Existing technology is difficult to effectively improve the hypoxic environment of wounds, resulting in limited wound healing, and the problem of antimicrobial resistance has not been effectively solved.
Develop a gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing that utilizes photothermal and photodynamic therapy through liposome-encapsulated perfluorodecalin nanoparticles and Cypate-linked antimicrobial peptides, combined with recombinant type III collagen gelatin Synergistically sterilizes and releases antibacterial components in the microenvironment to improve hypoxia.
The dressing not only improves the hypoxic environment of the wound while being highly antibacterial, promotes cell proliferation and tissue regeneration, accelerates wound healing, and reduces the biological toxicity of antimicrobial peptides, but also has a simple preparation process, low cost, and is suitable for large-scale production.
Smart Images

Figure BDA0003949434440000061 
Figure BDA0003949434440000151 
Figure HDA0003949434450000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nanomedical materials, and particularly relates to a gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing and a preparation method thereof. Background Art
[0002] As the first line of defense of the human body, the skin plays an irreplaceable role in resisting bacterial infections. Therefore, wound infections caused by skin damage, especially the emergence of drug resistance and antibiotic resistance, seriously threaten human life and health. The discovery and subsequent application of antibiotics in clinical practice have completely changed medicine and the treatment of bacterial infections. With the widespread use of antibiotics, bacterial resistance to antibiotics has increased. Antimicrobial peptides (AMPs), as a new type of broad-spectrum antibacterial agent, have attracted much attention from researchers due to their good antibacterial effects and unique antibacterial mechanisms.
[0003] Cypate is a carboxyl derivative of ICG (indocyanine green) with excellent photothermal conversion performance and is a commonly used photothermal compound. Due to the lack of active groups, ICG can only be connected to proteins by non-covalent bonds, and its stability is poor. Cypate is highly hydrophobic and has better structural stability. In addition, there are two carboxyl groups in its structure, which can react with the amino groups in the amino acid structure to form a covalent bond.
[0004] Oxygen is essential for human life activities. It produces a large amount of adenosine triphosphate (ATP) through aerobic glycolysis. Oxygen also plays a key role in wound healing because repair processes, such as attacking bacteria, cell proliferation, and collagen synthesis during the inflammatory stage, require a lot of energy. However, the oxygen content in the necrotic area of wound tissue is usually less than 10 mmHg (the transcutaneous oxygen content of normal tissue can reach 40 mmHg). Existing methods, such as hyperbaric oxygen therapy or local oxygen therapy, are difficult to alleviate the hypoxia of the wound environment. Therefore, there is an urgent need for a new material that can be applied to wounds to directly provide oxygen to wound cells, so as to improve the problem of hypoxia in wound tissue and provide favorable conditions for wound healing.
[0005] Organic compounds containing fluorine atoms can replace blood in the blood to transport oxygen, and perfluorodecalin (FDC) is one of the fluorine-containing compounds that can transport oxygen. Perfluorodecalin (FDC) is a perfluorocarbon compound with excellent oxygen carrying capacity and a suitable half-life in the body (about 6 hours), and is an excellent artificial blood substitute. However, due to the extreme hydrophobicity of FDC, its application is limited. Summary of the invention
[0006] The purpose of the present invention is to provide a gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing GCACF, which can not only effectively resist bacteria, but also improve the wound hypoxia microenvironment and promote wound healing, and a preparation method thereof. The hydrogel wound dressing prepared by the present invention can respond to the release of gelatinase, while synergizing with photothermal and photodynamic therapy to eradicate bacteria, and can significantly improve cellular hypoxia in in vitro experiments.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing provided by the invention is composed of liposome-encapsulated perfluorodecalin nanoparticles (FL), Cypate-connected antimicrobial peptides (AC) and gelatin added with recombinant type III collagen.
[0009] Among them, the antimicrobial peptide sequence is KKLRLKIAFK, which was synthesized by solid phase synthesis;
[0010] The maximum absorption band of Cypate is 780nm.
[0011] The antimicrobial peptide linked to Cypate is formed by covalently linking the carboxyl group in Cypate and the free amino group of the antimicrobial peptide amino acid, and its maximum absorption peak is 780 nm, which is consistent with the absorption peak of Cypate.
[0012] Liposome-encapsulated perfluorodecalin nanoparticles were prepared by ultrasonic emulsion method, and their hydrated particle size was stable at 350nm, the potential was -5mV, and they had excellent oxygen carrying capacity.
[0013] The hydrated particle size of the liposome nanoparticles alone was 100 nm and the potential was -45 mV.
[0014] The gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing GCACF is prepared by a one-pot method, wherein AC, FL, ColⅢ and gelatin (Gel) are heated and stirred together. The specific preparation method is as follows:
[0015] Type A gelatin was dissolved in FL solution at 40°C and stirred at 300 r / min for 30 min. Then, AC, ColⅢ and 10% glutamine transaminase were added to the above solution, stirred for 15 min, cooled to gel, and stored in a refrigerator at 4°C for later use. The hydrogel dressing obtained by this method is referred to as GCACF.
[0016] The above-mentioned gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing GCACF can not only degrade and release the antibacterial component AC in the microenvironment where Staphylococcus aureus exists, but also use the photothermal properties of Cypate and photodynamic therapy to synergistically kill bacteria under the action of near-infrared.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The hydrogel wound dressing obtained by the present invention can not only respond to microenvironmental release, but also improve the wound hypoxic microenvironment while being highly effective in antibacterial, promoting cell proliferation and tissue regeneration, thereby accelerating wound healing.
[0019] (2) The hydrogel wound dressing obtained by the present invention can respond to microenvironmental release, and has photothermal and photodynamic synergistic antibacterial effects, which reduces the amount of antimicrobial peptides used. The sustained release effect of the hydrogel greatly reduces the biological toxicity of the antimicrobial peptides.
[0020] (3) The hydrogel wound dressing of the present invention has a simple preparation process, low cost, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is the structural formula of the antibacterial short peptide KKLRLKIAFK;
[0022] Figure 2 The gelling properties of GCACF at different temperatures after treatment with different volumes of 10% glutamine aminotransferase;
[0023] Figure 3 HPLC analysis spectra of AMP, Cypate and AC;
[0024] Figure 4 is the mass spectrum of AMP and AC;
[0025] Figure 5 is the transmission electron microscope (TEM) image of FL;
[0026] Figure 6 is the hydrated particle size of Lip and FDC@Lip (where the left side is Lip and the right side is FDC@Lip);
[0027] Figure 7 The changes of hydrated particle size on the first and seventh days of FL;
[0028] Figure 8 The potential change diagram and solution appearance change diagram of Lip and FDC@Lip;
[0029] Fig. 9 Scanning electron microscope (SEM) image of gelatin hydrogel (GC) with ColⅢ added;
[0030] Fig.10 is the scanning electron microscope (SEM) image of GCACF;
[0031] Fig.11 It is the picture of the gelation of hydrogels with different components;
[0032] Fig.12 The fluid dynamics performance pictures of GC and GCACF;
[0033] Fig.13 is the UV-visible absorption spectrum of AC;
[0034] Fig.14 is the standard curve of AC concentration;
[0035] Fig.15 This is the temperature rise curve of AC with the same concentration and different photothermal powers;
[0036] Fig.16 This is the temperature rise curve of AC with the same photothermal power and different concentrations;
[0037] Fig.17 is the photothermal heating curve of GCACF;
[0038] Fig.18 This is a graph of the production of reactive oxygen species by AC under near-infrared light (from top to bottom, 0 to 10 min);
[0039] Fig.19 This is a comparison chart of the oxygen carrying capacity of water, Lip and FL;
[0040] Fig. 20 The graph shows the bactericidal effect of different concentrations of AC on S. aureus;
[0041] Fig.21 The graph shows the bactericidal effect of different concentrations of AC on E.coil;
[0042] Fig. 22 This is the sterilization effect of AC of different concentrations on S. aureus after near-infrared light irradiation;
[0043] Fig.23 This is the sterilization effect of AC of different concentrations on E.coil after near-infrared light irradiation;
[0044] Fig.24 The growth curve inhibition graph of AC on S. aureus and E. coil;
[0045] Fig.25 The figure shows the inhibition and destruction of S. aureus biofilm by AC;
[0046] Fig.26 The figure shows the sterilization effect of different material components on S. aureus and E. coil;
[0047] Fig. 27 Live / Dead staining images before and after the action of GCACF on S. aureus;
[0048] Fig.28 is the hemolysis rate graph;
[0049] Fig.29 This is a graph of cytotoxicity experiment data;
[0050] Fig.30 This is a graph showing the material's effect on the recovery of hypoxic cell viability;
[0051] Fig.31 This is the Western Blot experimental data graph;
[0052] Fig.32 This is a diagram showing the treatment of S. aureus infected mouse wound model by GCACF;
[0053] Fig.33 Plate image of mouse wound tissue;
[0054] Fig.34 H&E, Masson, and CD31 immunohistochemical staining of wound tissues;
[0055] Fig.35 Tissue sections of mouse heart, liver, spleen, lung, and kidney;
[0056] Fig.36 The results of the biocompatibility test of the drug-loaded hydrogel (4 mg AMP-Cypate) in comparison with Example 1 on L929 cells are shown in FIG.
[0057] Fig.37 This is a graph comparing the bactericidal effects of different concentrations of drug-loaded hydrogels on S. aureus in Example 1. DETAILED DESCRIPTION
[0058] The present invention is described in detail below with reference to the examples, but these examples are only for illustration and should not be construed as limiting the implementation of the present invention.
[0059] Example 1
[0060] 1. Preparation of enzyme-responsive photothermal oxygen-carrying hydrogel wound dressing GCACF
[0061] 1) Synthesis of Cypate-coupled antimicrobial peptide (AC)
[0062] The combination of cypate and antimicrobial peptide is achieved by reacting the carboxyl group on cypate with the amino group on the antimicrobial peptide to form a covalent bond. HoBt inhibits racemization in peptide synthesis, and EDC acts as a carboxyl activator to catalyze the reaction. The specific steps are as follows:
[0063] AMPs (KKLRLKIAFK) was synthesized using the Fmoc solid phase synthesis method with Rink Amide-MBHA resin as a carrier. After the peptide sequence was synthesized, the Fmoc protecting group was removed using a 20% piperidine solution, and 5 equivalents of Cypate and 1.2 equivalents of EDC and HoBT were added. DMF was used as a solvent and the reaction was carried out at room temperature in the dark overnight. Then, a cutting solution (TFA, EDT, H2O and TIS (94:2.5:2.5:1, v / v / v / v)) was added. After three hours of reaction, the peptide was cut from the resin. Subsequently, icy ether was added to precipitate AMP-Cypate, centrifuged, and the precipitate was purified by HPLC and measured by LC-MS.
[0064] 2) Preparation of FDC@Lip(FL)
[0065] The preparation of FL nanoparticles adopts the ultrasonic emulsion method, and the particle size and stability of the nanoparticles are studied by controlling the dosage ratio of soybean lecithin and cholesterol. The specific implementation process is as follows:
[0066] a) Dissolve soybean lecithin and cholesterol in 5 mL of chloroform at a ratio of (12:1 m / m) and mix well. Then remove the chloroform using a rotary evaporator, add appropriate amount of water (3 mg / mL), 0.08 times the amount of ethanol and 0.16 times the amount of FDC. Place the system in a cell ultrasonic disruptor, protect with low temperature nitrogen, and ultrasonicate for 15 minutes.
[0067] b) Dissolve soybean lecithin and cholesterol in 5 mL of chloroform at a ratio of (10:1 m / m) and mix well. Then remove the chloroform using a rotary evaporator, add appropriate amount of water (3 mg / mL), 0.08 times the amount of ethanol and 0.16 times the amount of FDC. Place the system in a cell ultrasonic disruptor, protect with low temperature nitrogen, and ultrasonicate for 15 minutes.
[0068] c) Dissolve soybean lecithin and cholesterol in 5 mL of chloroform at a ratio of (8:1 m / m) and mix well. Then remove the chloroform using a rotary evaporator, add appropriate amount of water (3 mg / mL), 0.08 times the amount of ethanol and 0.16 times the amount of FDC. Place the system in a cell ultrasonic disruptor, protect with low temperature nitrogen, and ultrasonicate for 15 minutes.
[0069] d) Dissolve soybean lecithin and cholesterol in 5 mL of chloroform at a ratio of (6:1 m / m) and mix well. Then remove the chloroform using a rotary evaporator, add appropriate amount of water (3 mg / mL), 0.08 times of ethanol and 0.16 times of FDC. Place the system in a cell ultrasonic disruptor, protect with low temperature nitrogen, and ultrasonicate for 15 minutes.
[0070] Table 1
[0071]
[0072] The particle size of the FL nanoparticles prepared by schemes a, b, c, and d was measured by a Malvern particle size analyzer. Each sample was measured three times in parallel and the average value was taken. The results are shown in Table 1. It can be seen that the particle size and PDI of the nanoparticles obtained when the mass ratio of soybean lecithin to cholesterol is 10:1 are the smallest. This shows that the nanoparticles have good dispersibility and are of appropriate size.
[0073] 3) Preparation of GCACF
[0074] Take 1g of type A gelatin, add 10mL of FDC@Lip, and melt the gelatin in a 40℃ water bath. Then add 0.2g of recombinant type III collagen (ColⅢ), continue stirring to dissolve it, add 100μL of 1000μM AC solution and 1mL of 10% glutamine transaminase and stir evenly to ensure that the final concentration of AC in the whole system is 10μM, let it stand for 1h to gel by itself, obtain ACGCF, and store it in a 4℃ refrigerator for later use. Because it is enzyme-linked gelation, the effect of the amount of glutamine transaminase on gelation was explored before, and finally 1mL was selected. The results are shown in Table 3 and Figure 2 shown.
[0075] Table 2 shows the dosage of 10% glutamine transaminase
[0076] Serial number Dosage / mL ① 1.2 ② 1 ③ 0.5 ④ 0.2 ⑤ 0
[0077] Table 3 shows the gelation of GCACF hydrogels with different ratios at different temperatures
[0078] Temperature / ℃ ① ② ③ ④ ⑤ 25 √ √ √ √ √ 30 √ √ √ √ √ 35 √ √ √ √ × 40 √ √ √ × × 45 √ √ × × × 50 √ √ × × × 55 √ √ × × ×
[0079] (√: gelled ×: not gelled)
[0080] 2. Preparation of drug-free hydrogel GC and Gel@ColⅢ+FDC@Lip(GCF).
[0081] According to the dosage of drug-loaded hydrogel, 1g type A gelatin and 0.2g ColⅢ were added, dissolved in 10mL water at 40°C, 1mL 10% glutamine transaminase was added, and the mixture was allowed to stand for 1h to crosslink into gel (non-drug-loaded hydrogel GC).
[0082] Preparation of Gel@ColⅢ+FDC@Lip(GCF).
[0083] Take 1g of type A gelatin, add 10mL of FDC@Lip, and melt the gelatin in a 40℃ water bath. Then add 0.2g of recombinant type III collagen (ColⅢ) and 1mL of 10% glutamine transaminase, stir evenly to dissolve, and let stand for 1h to form gel (Gel@ColⅢ+FDC@Lip).
[0084] 3. Characterization of enzyme-responsive photothermal oxygen-carrying hydrogel wound dressing GCACF
[0085] 1) Characterization of AC
[0086] Take 5 mg of AMP and AC and dissolve them in ultrapure water, and dissolve Cypate in acetonitrile and water, and use high performance liquid chromatography and mass spectrometry to verify compound AC. The results are as follows Figure 3 , Figure 4 Shown: Through Figure 3 It can be seen that AMP alone has no absorption peak at 700 nm, Cypate has an absorption peak at 700 nm, and AMP coupled with Cypate has an absorption peak at 700 nm, and the absorption peak position is shifted. Figure 4 The mass spectrum of AMP and Cypate can prove the successful coupling.
[0087] 2) Determination of hydrated particle size and appearance of FL
[0088] After the synthesized FL was diluted 10 times with ultrapure water, each sample was measured three times in parallel, and the average value was taken. The distribution of hydrated particle size and appearance morphology were measured using a Malvern particle size analyzer and a transmission electron microscope. Figure 5 , Figure 6 As shown: FL nanoparticles have good dispersibility and the particle size distribution is around 350nm. At the same time, it can be found that the particle size of the liposome alone is as small as about 100nm. After encapsulating perfluorodecalin, it becomes larger and then combined with Figure 8 The changes in the potential and appearance of the system preliminarily proved that perfluorodecalin was encapsulated in the liposomes. Figure 7 This indicates that FL nanoparticles have good stability.
[0089] 3) Characterization of GCACF
[0090] After freeze-drying GCACF, the morphology of GCACF was observed using a scanning electron microscope. Fig. 9 , Fig.10 As shown: The hydrogel is porous. After drug loading, the porosity phenomenon is significantly reduced. Fig.11 ), it can be found that the various components are fused with each other. The gelling properties of GCACF hydrogel were evaluated by rheometer. The test results are shown in Fig.12 , whether it is GC alone or after drug loading, the storage modulus of the hydrogel is always greater than the loss modulus, indicating that the hydrogel has good gelation properties.
[0091] 4. Study on the photothermal and photodynamic properties of AC and GCACF
[0092] Take 300 μL of 10 μM AC aqueous solution in 2 mL centrifuge tubes and use different powers (0.5 W / cm 2 , 1.0W / cm 2 , 1.5W / cm 2 , 2.0W / cm 2 )Near infrared laser irradiation for 5 min. The heating curves of different concentrations were similar. At a power of 1.5 W / cm 2 The temperature rise curves of AC aqueous solutions with different concentrations (0 μM, 2 μM, 4 μM, 6 μM, 8 μM, and 10 μM) were tested. Fig.15 , Fig.16 As shown, AC has good photothermal properties. The same method was then used to verify the photothermal properties of GCACF. The results are shown in Fig.17 As shown, GCACF also has excellent photothermal properties. DPBF was then used to measure the photodynamic properties of AC. DPBF (1,3-diphenylisobenzofuran) has an absorption peak at around 415nm. DPBF has high specificity for singlet oxygen, can form endoperoxides and decompose into 1,2-diphenylformylbenzene, resulting in a decrease in its absorption peak. Mix 1mL AC and 1mL DPBF in a quartz dish, wrap with tin foil to avoid light, and irradiate with an 808nm near-infrared laser (1.5W / cm 2 ), and tested every 1 minute. The results are as follows Fig.18 As shown, in the first two minutes, the absorption peak of DPBF decreased significantly, indicating that a large amount of singlet oxygen was generated, and AC had obvious photodynamic properties, which could synergistically kill bacteria.
[0093] 5. Study on the oxygen carrying capacity of FL
[0094] A handheld electrode dissolved oxygen meter was used to detect the change in oxygen content of FL. The specific steps are as follows: 5 mL of water, 5 mL of Lip solution, and 5 mL of FL were taken in 10 mL centrifuge tubes. Pure oxygen was introduced into the three solutions for 5 minutes, and then the handheld electrode dissolved oxygen meter was used to measure the change in oxygen content. The results were as follows: Fig.19 As shown, both the initial oxygen loading and the oxygen loading after stabilization in FL were higher than those in the control group, indicating that FL had a relative oxygen carrying capacity.
[0095] 6. In vitro antibacterial test of AC
[0096] 1) No near-infrared photothermal AC bacterial plating experiment
[0097] Use sterile water to prepare AC solutions with concentrations of 4, 8, 12, 16, and 20 μM, respectively. 8100 μL of S. aureus bacterial solution with CFU / mL was incubated with 100 μL of AC solution of different concentrations for 1 hour (the actual working concentration of AC is about 2, 4, 6, 8, 10 μM). 100 μL of PBS solution was used as a negative control. After the incubation, 100 μL was diluted 20,000 times and then spread on the plate. The plate was placed in a biochemical incubator (37°C) and cultured overnight. The number of colonies grown on the TSA plate was counted and each sample was measured three times in parallel. The E. coli was treated in the same way as above. The results are as follows Fig. 20 , Fig.21 As shown in the figure, it can be seen that the MIC90 of AC against S. aureus is about 8μM, and the MIC value against E. coil is about 15μM.
[0098] 2) Near infrared photothermal AC bacterial plate experiment
[0099] Use sterile water to prepare AC solutions with concentrations of 4, 8, 12, 16, and 20 μM, respectively. 8 100 μL of S. aureus bacterial solution with CFU / mL was mixed with 100 μL of AC solution of different concentrations, and then irradiated with near-infrared light using an 808 nm laser for 5 minutes and incubated together for 1 hour (the actual working concentration of AC is approximately 2, 4, 6, 8, and 10 μM). 100 μL of PBS solution was used as a negative control. After the incubation, 100 μL was diluted 20,000 times and spread on the plate. The plate was then placed in a biochemical incubator (37°C) and cultured overnight. The number of colonies grown on the TSA plate was counted, and each sample was measured three times in parallel. The E. coli was treated in the same manner as above. The results are as follows: Fig. 22 , Fig.23 As shown. After photothermal treatment, the antibacterial activity of AC against Staphylococcus aureus and Escherichia coli was significantly improved. The MIC90 of AC against S. aureus was about 2μM, and the MIC value against E.coil was about 5μM. The antibacterial effect was significantly improved.
[0100] 3) Growth curve determination of AC
[0101] In order to study the effect of AC on the growth of the two bacteria, the overnight cultured S. aureus and E. coli were diluted to 10 5 CFU / mL, 100 μL of bacterial solution was added to each 96-well plate, and 100 μL of 4 μM and 10 μM AC solution (actual working concentrations were 2 μM and 5 μM) were added respectively, and the plates were divided into 6 groups: S. aureus + PBS group, S. aureus + AC group, S. aureus + AC + IR group, E. coli + PBS group, E. coli + AC group, and E. coli + AC + IR group. Five wells in each group were used as parallel samples. The 808 nm laser (1.5 W / cm 2) The light-exposed group was irradiated for 5 minutes, and the group without laser irradiation and PBS solution was used as the control group. The absorbance of each well at 600 nm was detected and recorded every hour using an ELISA reader, and the monitoring was continued for 12 hours. The growth curves of bacteria in the experimental group and the control group were plotted based on the measured data. The results are shown in Fig.24 The results were consistent with the results of the plate coating. After adding near-infrared light, the bacterial growth was significantly inhibited.
[0102] 4) AC inhibits and destroys Staphylococcus aureus biofilm
[0103] a. Inhibition of biofilm
[0104] A flat-bottom 96-well plate was selected, and 100 μL of S. aureus in the logarithmic growth phase was added to the selected 9 wells. The plates were divided into 3 groups: PBS control group, AC group, and AC+NIR (808 nm laser irradiation for 5 min) group. The final volume of each group was 200 μL and the actual working concentration of AC was 4 μM. Three parallel samples were set up in each group. The illumination group used an 808 nm laser (1.5 W / cm 2 ) irradiation for 5 minutes. Place the 96-well plate in a biochemical incubator at 37°C and incubate for 48 hours. After the incubation is completed, use a pipette to slowly aspirate the upper culture medium, wash the wells with PBS 2-3 times, air-dry for 10 minutes, and then add 100 μL of 1% crystal violet solution to each well for staining for 20 minutes. After the staining is completed, slowly and gently use a pipette to aspirate the crystal violet solution along the wall, wash the selected wells with sterile PBS 3 times, and then air-dry for 10 minutes. Add 200 μL of 80% ethanol to each experimental well, place the 96-well plate in a constant temperature shaker and shake until the crystal violet is completely dissolved, use an enzyme reader to detect the absorbance of each well at 590nm, take the average value and record the data. The results are as follows Fig.25 As shown in (left), it can be seen that AC can inhibit the biofilm formation of S. aureus. After near-infrared light irradiation, the effect is more obvious, which is consistent with the trend of previous experimental results.
[0105] b. Destruction of biofilm
[0106] A flat-bottomed 96-well plate was selected, and 100 μL of S. aureus in the logarithmic growth phase was added to the selected 9 wells. The 96-well plate was placed in a biochemical incubator at 37°C for 48 hours to allow the biofilm to grow. The biofilms were then divided into three groups: PBS control group, AC group, AC+NIR (808nm 1.5W / cm 2 The final volume of each group was 200 μL and the actual working concentration of AC was 4 μM. Three parallel samples were set up in each group. The illumination group used an 808 nm laser (1.5 W / cm 2) irradiation for 5 minutes. Place the 96-well plate in a biochemical incubator at 37°C and incubate for 1 hour. After the incubation is completed, use a pipette to slowly aspirate the upper culture medium, wash the wells with PBS 2-3 times, air-dry for 10 minutes, and then add 100 μL of 1% crystal violet solution to each well for staining for 20 minutes. After the staining is completed, slowly and gently use a pipette to aspirate the crystal violet solution along the wall, wash the selected wells with sterile PBS 3 times, and then air-dry for 10 minutes. Add 200 μL of 80% ethanol to each experimental well, place the 96-well plate in a constant temperature shaker and shake until the crystal violet is completely dissolved, use an enzyme reader to detect the absorbance of each well at 590nm, take the average value and record the data. The results are as follows Fig.25 As shown in (right), AC also has a destructive effect on existing biofilms, and the effect is more obvious after near-infrared light irradiation.
[0107] 5) GCACF antibacterial coating
[0108] Take 10 8 100 μL of S. aureus bacterial solution with CFU / mL was incubated with 100 μL of GCACF and AC solution for 3 h (the actual working concentration of AC is about 4 μM). 100 μL of PBS solution was used as negative control, and the illumination group was illuminated with 808 nm laser for 5 min (power of 1.5 W / cm 2 ). After the incubation, 100 μL of the solution was diluted 20,000 times and plated, and then placed in a biochemical incubator (37°C) for overnight culture. The number of colonies grown on the TSA plate was counted, and each sample was measured three times in parallel. The E. coli was treated in the same way as above. The results are shown in the figure. Fig.26 Compared with Escherichia coli, Staphylococcus aureus is more sensitive to GCACF hydrogel, which is related to the ability of Staphylococcus aureus to secrete gelatinase, which can degrade gelatin and release the antibacterial material AC in it to achieve the purpose of sterilization.
[0109] 6) Bacterial live and dead staining
[0110] The effect of GCACF photothermal treatment on the viability of Staphylococcus aureus was studied by live / dead staining. 100 μL of GCACF was added to 100 μL of 10 8 CFU / mL of S. aureus, and then incubated for 30 min with a near-infrared laser (808 nm, 1.5 W / cm 2) irradiated the bacteria for 10 minutes. The three groups of samples were centrifuged at 5000rpm for 10 minutes, the supernatant was discarded, and the precipitate was stained with 30μL live / dead reagent, pipetted evenly, vortexed and kept in the dark for 20 minutes. Finally, 20μL of the sample was dropped on a slide and observed with an inverted fluorescence microscope. According to the manufacturer's instructions, live bacterial cells were stained with SYTO 9 dye (green), while dead bacterial cells were labeled with propidium iodide dye (red) due to damaged cell walls and cell membranes. The results are shown in Fig. 27 As shown in the figure, under near-infrared light irradiation, the red fluorescence emitted was the most, while the PBS group almost only showed green light despite the addition of near-infrared irradiation. This shows that GCACF can perform photothermal and photodynamic synergy and has excellent photothermal antibacterial effect.
[0111] 7. GCACF hemolysis test
[0112] Fresh mouse blood was centrifuged (300rmp / min) for 5 minutes and then red blood cells were collected. After centrifugation, the red blood cells were washed three times with sterile PBS (0.1M, pH=7.4). The purified red blood cells were diluted with PBS to a concentration of 20%. Then 20 μL of red blood cells were incubated with different concentrations of AC and GCACF in a centrifuge tube in an incubator (37°C). PBS and 1% Triton solution were used as negative and positive controls, respectively. In order to eliminate the interference of AC on blood absorption, PBS was mixed with AC and the absorbance was measured as follows. The hemolysis rate was calculated as follows:
[0113] Hemolysis rate (%) = (A1-A2-A3) / (A4-A3)
[0114] A1, A2, A3, and A4 are the absorbance values of the sample to be tested, AC of the same concentration, negative control, and positive control, respectively.
[0115] The results are as follows Fig.28 As shown, the results showed that when the AC concentration was 2.5 μM, the hemolysis rate was about 10%, but the hemolysis rate of GCACF when the AC concentration was 10 μM was about 3%, indicating that GCACF hydrogel can significantly improve the hemolysis rate and biological toxicity of AC.
[0116] 8.GCACF Cytotoxicity Experiment
[0117] L929 cells were used as experimental materials, and the MTT method was used to detect the cytotoxicity of GCACF hydrogel and its components. First, L929 cells were revived, replaced with medium, and subcultured, and the experiment was carried out when the cell viability was good. In the formal experiment, L929 cells were seeded on a 96-well microplate (10 cells per well). 4The cells were incubated overnight with different materials and the uninoculated pores were filled with sterile PBS. After 24 h of incubation, MTT assay was performed and the absorbance of L929 cells at 490 nm was measured with a microplate reader to evaluate the cytotoxicity of the hydrogel and its components, thereby studying the cell viability. The results are shown in Fig.29 As shown, AC alone was highly toxic to cells, and cell survival was only about 60% of that in the control group, while cells in the GC and GCACF groups were not affected, and the survival rate did not change significantly compared with the control group. In the FL group, the cell survival rate was significantly improved compared with the control group, which was related to the fact that FL carried oxygen and promoted cell growth. These results show that GCACF has good biocompatibility.
[0118] 9. GCACF recovery experiment on hypoxic cells
[0119] In this study, L929 cells were used as experimental materials, and the MTT method was used to detect the effects of GCACF hydrogel and its components on hypoxic cells. First, L929 cells were seeded on a 96-well plate (10 cells per well). 4 The cells were incubated overnight with 600 μM CoCl2 and incubated for 12 h to induce hypoxia. GCACF hydrogel and its components were then added and incubated at 37°C for 24 h. MTT assay was performed and the absorbance of L929 cells at 490 nm was measured with a microplate reader to evaluate the effects of the hydrogel and its components on hypoxic cells. The results are shown in Figure 2. Fig.30 As shown, the AC group had no improvement on hypoxic cells. The FL group and GCACF group had a certain improvement on hypoxic cells due to the presence of FL nanoparticles, and the GC group had a promoting effect on cell growth due to the addition of recombinant collagen.
[0120] 10.Western Blot (WB) experiment
[0121] In order to further explore the effects of hydrogel and its components on hypoxic cells, WB experimental technology was used to perform qualitative and quantitative analysis of hypoxia inducible factor (HIF) expressed by hypoxic cells. The specific experimental steps are as follows:
[0122] 1) First, prepare the separation gel and the concentration gel according to Table 4;
[0123] 2) Sample preparation: Add 600 μM CoCl2 and the sample group to the cell suspension and culture for 12 hours. Scrape the cells into a centrifuge tube, lyse them in an ice bath with cell lysis buffer for 1 hour, and centrifuge to obtain the supernatant. Use a BCA protein kit to determine the protein concentration and add 5X loading buffer (working concentration is 1X);
[0124] 3) Gel running: 80V, 30min; 110V, 150min; according to the mark, cut the bands near 120KDa and 36KDa;
[0125] 4) Transfer: Activate the PVDF membrane with methanol in advance; place the sandwich board with the black side facing down, and arrange it in the order of sponge pad, filter paper, glue, PVDF membrane, filter paper, and sponge pad. Perform low-temperature transfer at 120V for 45min;
[0126] 5) Blocking: Shake with 5% skim milk powder for 1 hour to block the unbound sites on the PVDF membrane;
[0127] 6) Incubation with primary antibodies: Add the corresponding rabbit primary antibodies of HIF-α and GADPH, respectively, and incubate in a refrigerator at 4°C overnight;
[0128] 7) Incubation with secondary antibody: Recover the primary antibody, wash with TBST for 3×10 min, add rabbit secondary antibody, and incubate at room temperature for 1 h;
[0129] 8) Development: ECL developer is used for development and exposure.
[0130] The results are as follows Fig.31 It can be found that the HIF-1α protein expressed in the GCACF group is less than that in the hypoxia control group, and the HIF-1α protein expressed in the FL group is even less than that in the control group. This shows that FL can significantly improve cell hypoxia, and the GCACF hydrogel with FL added also has a certain effect in improving cell hypoxia.
[0131] Table 4
[0132]
[0133] 11. GCACF for the study of Staphylococcus aureus infection
[0134] 1) Establishment of Staphylococcus aureus skin infection model
[0135] The specific modeling method is as follows: the back of Balb / c mice was shaved to expose the skin overnight, and the next day, an elliptical full-thickness wound was constructed on the back using a hole punch, with a long axis of about 8 mm and a short axis of about 6 mm; then 20 μL of Staphylococcus aureus solution (10 8 CFU / mL) overnight, and to ensure successful infection, infection was performed twice.
[0136] 2) Treatment of wounds infected with Staphylococcus aureus
[0137] In order to explore the treatment effect of GCACF on bacterial infection wounds, the experimental mice with established models were divided into 7 groups, including GCACF, GCACF+IR (1.5W / cm 2, 5min), AC, AC+IR (1.5W / cm 2 , 5min), GC, FL and PBS, with 3 parallel samples in each group. Each mouse was raised individually to allow it to drink water and eat freely to eliminate other experimental interferences. The process was administered 4 times (once a day in the first 4 days). The mice in the light group were fixed with a fixing plate each time they were administered. The temperature was monitored using a thermal imager during the entire near-infrared process to ensure that the temperature was maintained at around 46°C to prevent the temperature from failing to meet the treatment requirements or being too high to damage normal tissues. Finally, in order to monitor the changes in the infected wound and the changes in the physical signs of mice during the treatment process, photos of the wound were taken every day. On the tenth day of treatment, the tissue site was disinfected with medical scissors and removed, and each group of tissues was preserved with an equal volume of sterile PBS for plating experiments. The bacterial plates were placed in an incubator at 37°C for overnight culture, and the number of colonies was measured. The wound healing effect and wound colony plating results are shown in Fig.32 , Fig.33 .
[0138] The experimental results show that the treatment effect of the GCACF+IR group is the closest. In the PBS group, there was still bacterial infection on the tenth day, and there was yellow pus under the scab of the wound. The GC group was similar to the PBS group because it did not have antibacterial ingredients and had no good effect on bacterial infection. In the FL group, oxygen can be transported to provide oxygen to immune cells during the inflammatory stage of wound healing, so that immune cells can play a better role and kill bacteria, so the healing situation is better than that of the PBS and GC groups. The AC group and the AC+IR group can kill bacteria efficiently. Due to the removal of bacteria, a better environment can be provided for wound healing, so the wound healing of the AC group and the AC+IR group is better. The wound healing of the GCACF group is also good. This is because the GCACF hydrogel material has both bactericidal and oxygen-carrying capabilities, which has a very good promoting effect on wound healing. Combined with the photothermal effect, it can further improve the speed of wound healing. It was basically healed on the 8th day and completely healed on the 10th day. At the same time, it can be seen from the results of the coating that no bacteria were found in the experimental group containing the AC component, indicating that the bacteria were effectively killed, while in other groups, there were bacteria, among which the PBS group had more, which is also consistent with the situation of wound healing. These results all indicate that GCACF hydrogel can provide oxygen to wounds and promote wound healing while effectively killing bacteria.
[0139] 3) Wound tissue sections
[0140] In order to verify the effect of the material on wound healing, the wound tissue was stained and evaluated. Fig.34. H&E staining showed that there was no new epidermis in the PBS group, GC group, and FL group. The GC+FL group, AC+IR group, and GCACF group had discontinuous new epidermis, while the GCACF+IR group had continuous new epidermis (arrows). At the same time, Masson staining and CD31 immunohistochemistry also showed the same wound healing trend. In Masson staining, the collagen deposition (blue) in the PBS group, GC group, and FL group was less and loose, and the collagen deposition in the GC+FL group increased, but not as much as that in the AC+IR group. The main reason was that the GC+FL group did not contain antibacterial materials. Although it could provide the required collagen and oxygen for wound healing, the remaining bacteria would interfere with the production of collagen and the normal healing of the wound. This can also be seen from the GCACF group and GCACF+IR group with the addition of antimicrobial peptides. The collagen fibers in the GCACF group and GCACF+IR group were thick and dense, with regular orientation and collagen network topology, which was consistent with the wound healing situation and showed a good healing state. CD31 immunohistochemistry verified the wound healing situation from the side. CD31 is a typical marker of endothelial cells and is usually associated with angiogenesis. The results showed that the GCACF+IR group had more new blood vessels (indicated by the arrows), indicating that the wound healing was better. Through the heart, liver, spleen, lung and kidney tissue sections of mice, it was found that there was no significant difference between the experimental group and the control group, indicating that the material was non-toxic to the main organs of mice ( Fig.35 ).
[0141] Comparative Example 1
[0142] Preparation of enzyme-responsive photothermal hydrogel
[0143] 4 mg AMP(LLKKLRLKIA)-Cypate was added to obtain GCACF (80 μM). The rest was the same as in Example 1. 1. Preparation of enzyme-responsive photothermal oxygen-carrying hydrogel wound dressing GCACF.
[0144] After dilution with DMEM medium, the concentrations (0μM, 2μM, 4μM, 6μM, 8μM) were obtained, and the results showed a certain growth effect ( Fig.36 ), but could not reach the antimicrobial concentration of antimicrobial peptides (10 μM) ( Fig.37 ), and therefore could not meet the concentration requirements of the cytotoxicity experiment (the upper limit needs to include the antibacterial concentration (10 μM)).
[0145] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A gelatinase-responsive photothermal oxygen-carrying hydrogel wound dressing, characterized in that: The preparation method of the gelatinase responsive photothermal oxygen-carrying hydrogel wound dressing comprises the following steps: (1) Perfluorodecahydronaphthalene FDC@Lip nanoparticles were prepared by ultrasonic emulsion method: 10 mg soybean lecithin and 1 mg cholesterol were dissolved in 5 mL chloroform respectively and mixed evenly. The chloroform was then removed by rotary evaporator, and water, 0.08 times the amount of ethanol and 0.16 times the amount of FDC were added. The system was placed in a cell ultrasonic disruptor, protected by low-temperature nitrogen, and ultrasonicated for 15 min. The amount of water added was such that the total mass concentration of soybean lecithin and cholesterol was 3 mg / mL. (2) Take 1 g of type A gelatin, add 10 mL of FDC@Lip, melt the gelatin in a 40°C water bath, then add 0.2 g of recombinant type III collagen Col Ⅲ, continue stirring to dissolve it, add 100 μL of 1000 μM Cypate-coupled antimicrobial peptide AC solution and 1 mL of 10% glutamine transaminase and stir evenly to ensure that the final concentration of AC in the entire system is 10 μM, let it stand for 1 hour to allow it to gel, and store it in a 4°C refrigerator for later use to prepare a hydrogel dressing; Among them, Cypate-coupled antimicrobial peptide AC is obtained by reacting the carboxyl group on Cypate with the amino group on the antimicrobial peptide to form a covalent bond; The antimicrobial peptide sequence is KKLRLKIAFK, and it was synthesized by solid phase method; The maximum absorption peak of cypate and antimicrobial peptides linked to cypate is 780 nm.