Preparation and application of a foamy spinel catalyst

The preparation of foam spinel-type catalyst with three-dimensional hierarchical pore structure by solvent-free melting method solves the problems of low specific surface area and poor anti-interference of spinel oxide catalysts, and achieves efficient removal of emerging organics in complex water environments Pollutants.

CN115920889BActive Publication Date: 2024-12-06SHANGHAI JIAOTONG UNIV
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202211384031.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-07
Publication Date
2024-12-06
Estimated Expiration
2042-11-07

AI Technical Summary

Technical Problem

The spinel-type oxide catalysts have low specific surface area and poor dispersion of active centers due to particle agglomeration, which reduces their catalytic performance, especially when natural organic matter is present.

Method used

The foam spinel-type catalyst with a three-dimensional hierarchical pore structure was prepared by solvent-free melting method, which increased the specific surface area and anti-interference ability, and achieved high selectivity to remove emerging organic pollutants in complex water environments.

Benefits of technology

The mass transfer efficiency and anti-interference of the catalyst are improved, the removal capacity of emerging organic pollutants is significantly improved, and the efficient preparation of the catalyst is achieved without consuming additional energy and solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115920889B_ABST
    Figure CN115920889B_ABST
Patent Text Reader

Abstract

The present invention discloses the preparation and application of a foamed spinel catalyst; the foamed spinel catalyst is mainly prepared by the following steps: 1) uniformly mixing a metal salt precursor and an organic matter in a certain proportion; 2) subjecting the system obtained in 1) to a calcination reaction; 3) grinding the system obtained in 2) to obtain a foamed spinel catalyst. The spinel catalyst prepared by the present invention has a three-dimensional hierarchical pore structure, which is not only conducive to the exposure of more active sites and the increase of mass transfer during the reaction, but also has a sieving effect based on pore size mediation, thereby greatly improving the ability of the catalyst to selectively remove emerging organic pollutants in a complex water environment. In addition, the preparation method of the present invention can realize the preparation of a foamed spinel catalyst in a short time without consuming additional energy and solvent, and is an environmentally friendly catalyst synthesis method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental material preparation, and in particular relates to the preparation and application of a foamed spinel catalyst. Background Art

[0002] In the past few decades, water pollution has become a serious environmental problem that affects our health. In order to effectively remove emerging organic pollutants (such as endocrine disruptors) from water, advanced oxidation technology based on persulfate activation has attracted widespread attention from researchers due to its low energy consumption and environmental protection.

[0003] So far, through the efforts of researchers, various persulfate catalysts for water pollution remediation have been developed, such as perovskite-type oxides, spinel-type oxide metal sulfides, layered double hydroxides, etc. Among these catalysts, spinel-type oxides (AB2O4) are considered to be promising persulfate catalysts due to their high stability and magnetic separability. However, AB2O4 particles are severely agglomerated, which leads to low specific surface area and poor dispersion of active centers, thereby reducing the number of active sites and reducing mass transfer efficiency. In addition, natural organic matter (NOM) (such as humic acid) is commonly present in natural water, which may cover the active sites on the catalyst surface, thereby significantly reducing its catalytic performance. Therefore, it is of great significance to develop spinel-type catalysts with many active sites and strong anti-interference. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing an efficient foamed spinel catalyst and its application. A foamed spinel catalyst with a three-dimensional hierarchical pore structure was successfully prepared by an environmentally friendly solvent-free melting method. The catalyst has a large specific surface area, which is beneficial to the exposure of active sites and the improvement of mass transfer efficiency. At the same time, due to the presence of the hierarchical pore structure, the spinel catalyst can also achieve highly selective degradation of emerging pollutants in the presence of NOM. More importantly, this method can achieve the preparation of a foamed spinel catalyst in a short time without consuming additional energy and solvents, and is an environmentally friendly catalyst synthesis method.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] The present invention relates to a foamed spinel catalyst, which is AB2O4, wherein A is a divalent metal and B is a trivalent metal; and has a three-dimensional hierarchical pore structure, including macropores and mesopores, the macropore size is 50-100nm, and the average mesopore diameter is 3.833nm. It not only has a large specific surface area to increase the exposure of active sites and improve mass transfer efficiency, but also its hierarchical pore structure can effectively screen natural organic matter, thereby greatly improving the catalyst's ability to selectively remove emerging organic pollutants in complex water environments.

[0007] The present invention also relates to a method for preparing a foamed spinel catalyst, comprising the following steps:

[0008] S1. Mix the metal salt precursor and the organic matter in a certain proportion;

[0009] S2, subjecting the system obtained in S1 to a calcination reaction;

[0010] S3. Grind the system obtained in S2 to obtain a foamy spinel catalyst.

[0011] The catalyst prepared by the preparation method of the present invention has a staggered three-dimensional structure, which can effectively block large molecular natural organic matter during water treatment, and then selectively degrade and remove small molecular emerging pollutants, which is the characteristic of the structure.

[0012] As an embodiment, in step S1, the metal salt precursor is at least one of nickel salt, copper salt, manganese salt, cobalt salt, aluminum salt, magnesium salt, iron salt and zinc salt.

[0013] As an embodiment, in step S1, the metal salt is at least one of nitrate, sulfate, acetate and chloride.

[0014] As an embodiment, in step S1, the organic matter is citric acid. Only when citric acid is used as the organic matter can a three-dimensional foamed spinel catalyst be obtained; if glucose is used, this purpose cannot be achieved.

[0015] As an embodiment, in step S1, the molar ratio of the organic matter to the metal salt precursor is 0:1-10:1.

[0016] As an embodiment, in step S2, the calcination temperature is 300-800°C.

[0017] As an embodiment, in step S2, the calcination time is 30-360 min.

[0018] As an embodiment, in step S2, the heating rate is 0.5-10°C / min.

[0019] As an embodiment, in step S2, the calcination atmosphere is air or pure oxygen.

[0020] The foamed spinel catalyst of the present invention and the use of the foamed spinel catalyst prepared by the above method in the activation of persulfate and the degradation of emerging organic pollutants also fall within the protection scope of the present invention.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1) The preparation of three-dimensional foamed spinel catalyst and the catalytic degradation of emerging organic pollutants in wastewater were achieved;

[0023] 2) In the three-dimensional foamed spinel catalyst, the large specific surface area is conducive to the exposure of active sites and the improvement of mass transfer efficiency, while the presence of the hierarchical pore structure enables the spinel catalyst to have good anti-interference properties, which greatly improves the ability of the catalyst to highly selectively remove emerging organic pollutants in complex water environments;

[0024] 3) The preparation method of the present invention can realize the preparation of a three-dimensional foamed spinel catalyst in a short time without consuming additional energy and solvent. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0026] Figure 1 Degradation diagram of foamed MnFe2O4 catalyst with different ratios of citric acid to metal salt, corresponding to the catalysts of Examples 1 to 5 (X is the molar ratio of citric acid to metal salt = 0.5:1-4.5:1);

[0027] Figure 2 Graph showing the effects of different systems on the degradation performance of emerging organic pollutants, corresponding to the catalysts of Example 3 and Comparative Example 1;

[0028] Figure 3 The SEM images of the foamed MnFe2O4 catalysts with different ratios of citric acid to metal salts correspond to the catalysts of Examples 1 to 5; wherein A is the SEM images at different magnification ratios when the molar ratio of citric acid to metal salt is 0.5:1; B is the SEM images at different magnification ratios when the molar ratio of citric acid to metal salt is 1.5:1; C is the SEM images at different magnification ratios when the molar ratio of citric acid to metal salt is 2.5:1; D is the SEM images at different magnification ratios when the molar ratio of citric acid to metal salt is 3.5:1; E is the SEM images at different magnification ratios when the molar ratio of citric acid to metal salt is 4.5:1;

[0029] Figure 4 It is a comparison diagram of the anti-interference performance of the foamed MnFe2O4 catalyst (MnFe2O4-S) and the granular MnFe2O4 catalyst (MnFe2O4-P), corresponding to Example 3 and Comparative Example 1;

[0030] Figure 5 : are SEM images of different foamy spinel catalysts, AD corresponds to the catalysts of Examples 6 to 9. DETAILED DESCRIPTION

[0031] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0032] Example 1

[0033] (1) 8 mmol of manganese acetate tetrahydrate, 16 mmol of ferric nitrate nonahydrate and 12 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0034] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0035] (3) Grinding the system obtained in (2) to obtain a foamed MnFe2O4 catalyst (CA / Metal=0.5);

[0036] (4) The prepared foamed MnFe2O4 catalyst (CA / Metal=0.5) was used to degrade bisphenol A in the presence of potassium persulfate complex salt to measure its catalytic activity. Figure 1 The degradation diagram of foamed MnFe2O4 catalyst with different ratios of citric acid to metal salt is shown in Figure 2. Figure 1 It can be found that the degradation rate of bisphenol A reaches 74.3% within 20 minutes. Figure 3 The SEM images of foamed MnFe2O4 catalysts with different ratios of citric acid to metal salts are shown in Figure 2. Figure 3 A shows that the prepared MnFe2O4 catalyst has a foamy structure.

[0037] Example 2

[0038] (1) 8 mmol of manganese acetate tetrahydrate, 16 mmol of ferric nitrate nonahydrate and 36 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0039] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0040] (3) Grinding the system obtained in (2) to obtain a foamed MnFe2O4 catalyst (CA / Metal=1.5);

[0041] (4) The prepared foamed MnFe2O4 catalyst (CA / Metal=1.5) was used to degrade bisphenol A in the presence of potassium persulfate complex salt to measure its catalytic activity. Figure 1 The degradation diagram of foamed MnFe2O4 catalyst with different ratios of citric acid to metal salt is shown in Figure 2. Figure 1 It can be found that the degradation rate of bisphenol A reaches 81.8% within 20 minutes. Figure 3 The SEM images of foamed MnFe2O4 catalysts with different ratios of citric acid to metal salts are shown in Figure 2. Figure 3 B shows that the prepared MnFe2O4 catalyst has a foamy structure.

[0042] Example 3

[0043] (1) 8 mmol of manganese acetate tetrahydrate, 16 mmol of ferric nitrate nonahydrate and 60 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0044] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0045] (3) Grinding the system obtained in (2) to obtain a foamed MnFe2O4 catalyst (CA / Metal=2.5) (MnFe2O4-S);

[0046] (4) The prepared foamed MnFe2O4 catalyst (CA / Metal=2.5) (MnFe2O4-S) was used to degrade bisphenol A in the presence of potassium persulfate complex salt to measure its catalytic activity. Figure 1 The degradation diagram of foamed MnFe2O4 catalyst with different ratios of citric acid to metal salt is shown in Figure 2. Figure 1 It can be found that the degradation rate of bisphenol A reaches 100.0% within 20 minutes. Figure 3 The SEM images of foamed MnFe2O4 catalysts with different ratios of citric acid to metal salts are shown in Figure 2. Figure 3 C shows that the prepared MnFe2O4 catalyst has a foamy structure.

[0047] The prepared foamed MnFe2O4 catalyst (CA / Metal = 2.5) (MnFe2O4-S) was mixed with potassium persulfate and 20 mg·L-1 The catalytic activity of bisphenol A was measured by degradation of bisphenol A in the presence of humic acid. Figure 4 Figure 4 is the degradation diagram of foamed MnFe2O4 catalyst and granular MnFe2O4 catalyst under different humic acid contents. It can be found from Figure 4 that in the presence of humic acid, the degradation rate of bisphenol A of MnFe2O4-S can reach 99.5% within 20 minutes.

[0048] The prepared foamed MnFe2O4 catalyst (CA / Metal = 2.5) (MnFe2O4-S) was mixed with potassium persulfate and 40 mg·L -1 The catalytic activity of bisphenol A was measured by degradation of bisphenol A in the presence of humic acid. Figure 4 Figure 4 is the degradation diagram of foamed MnFe2O4 catalyst and granular MnFe2O4 catalyst under different humic acid contents. It can be found from Figure 4 that the degradation rate of bisphenol A reaches 97.0% within 20 minutes.

[0049] Example 4

[0050] (1) 8 mmol of manganese acetate tetrahydrate, 16 mmol of ferric nitrate nonahydrate and 84 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0051] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0052] (3) Grinding the system obtained in (2) to obtain a foamed MnFe2O4 catalyst (CA / Metal=3.5);

[0053] (4) The prepared foamed MnFe2O4 catalyst (CA / Metal=3.5) was used to degrade bisphenol A in the presence of potassium persulfate complex salt to measure its catalytic activity. Figure 1 The degradation diagram of foamed MnFe2O4 catalyst with different ratios of citric acid to metal salt is shown in Figure 2. Figure 1 It can be found that the degradation rate of bisphenol A reaches 100.0% within 20 minutes. Figure 3 The SEM images of foamed MnFe2O4 catalysts with different ratios of citric acid to metal salts are shown in Figure 2. Figure 3 D shows that the prepared MnFe2O4 catalyst has a foamy structure.

[0054] Example 5

[0055] (1) 8 mmol of manganese acetate tetrahydrate, 16 mmol of ferric nitrate nonahydrate and 108 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0056] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0057] (3) Grinding the system obtained in (2) to obtain a foamed MnFe2O4 catalyst (CA / Metal=4.5);

[0058] (4) The prepared foamed MnFe2O4 catalyst (CA / Metal=4.5) was used to degrade bisphenol A in the presence of potassium persulfate complex salt to measure its catalytic activity. Figure 1 The degradation diagram of foamed MnFe2O4 catalyst with different ratios of citric acid to metal salt is shown in Figure 2. Figure 1 It can be found that the degradation rate of bisphenol A reaches 98.8% within 20 minutes. Figure 3 The SEM images of foamed MnFe2O4 catalysts with different ratios of citric acid to metal salts are shown in Figure 2. Figure 3 E shows that the prepared MnFe2O4 catalyst has a foamy structure.

[0059] Comparative Example 1

[0060] (1) The granular MnFe2O4 catalyst (MnFe2O4-P) was used to degrade bisphenol A in the presence of potassium persulfate complex salt to measure its catalytic activity. Figure 2 The effect of different systems on the degradation performance of emerging organic pollutants is shown in Figure 2. Figure 2 It can be found that the degradation rate of bisphenol A reaches 96.2% within 20 minutes, which is slightly lower than that of MnFe2O4-S, indicating that the unique foam structure is more conducive to the degradation of bisphenol A.

[0061] The granular MnFe2O4 catalyst (MnFe2O4-P) was mixed with potassium persulfate and 20 mg·L -1 The catalytic activity of bisphenol A was measured by degradation of bisphenol A in the presence of humic acid. Figure 4 Figure 4 shows the degradation diagram of foamed MnFe2O4 catalyst and granular MnFe2O4 catalyst under different humic acid contents. It can be found from Figure 4 that in the presence of humic acid, MnFe2O4-P can achieve a 73.2% degradation rate of bisphenol A within 20 minutes. However, compared with MnFe2O4-S, its degradation rate constant is more reduced, indicating that MnFe2O4-S has a certain anti-interference ability.

[0062] The granular MnFe2O4 catalyst (MnFe2O4-P) was mixed with potassium persulfate and 40 mg·L -1 The catalytic activity of bisphenol A was measured by degradation of bisphenol A in the presence of humic acid. Figure 4Figure 4 shows the degradation diagram of foamed MnFe2O4 catalyst and granular MnFe2O4 catalyst under different humic acid contents. It can be found from Figure 4 that in the presence of humic acid, MnFe2O4-P can achieve a 59.5% degradation rate of bisphenol A within 20 minutes. However, compared with MnFe2O4-S, its degradation rate constant is more reduced, further indicating that MnFe2O4-S has a certain anti-interference ability.

[0063] Example 6

[0064] (1) 8 mmol of cobalt acetate tetrahydrate, 16 mmol of ferric nitrate nonahydrate and 60 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0065] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0066] (3) The system obtained in (2) is ground to obtain a foamed CoFe2O4 catalyst (CoFe2O4-S). Figure 5 are SEM images of different foamy spinel catalysts. Figure 5 It can be seen that the CoFe2O4 catalyst also has a foamy structure.

[0067] Example 7

[0068] (1) 8 mmol of copper acetate monohydrate, 16 mmol of ferric nitrate nonahydrate and 60 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0069] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0070] (3) Grind the system obtained in (2) to obtain a foamed CuFe2O4 catalyst (CuFe2O4-S). Figure 5 are SEM images of different foamy spinel catalysts. Figure 5 It can be seen that the CuFe2O4 catalyst also has a foamy structure.

[0071] Example 8

[0072] (1) 8 mmol of nickel acetate tetrahydrate, 16 mmol of ferric nitrate nonahydrate and 60 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0073] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0074] (3) Grind the system obtained in (2) to obtain a foamed NiFe2O4 catalyst (NiFe2O4-S). Figure 5 are SEM images of different foamy spinel catalysts. Figure 5 It can be seen that the NiFe2O4 catalyst also has a foamy structure.

[0075] Example 9

[0076] (1) 8 mmol of zinc acetate dihydrate, 16 mmol of ferric nitrate nonahydrate and 60 mmol of citric acid monohydrate were placed in a crucible and mixed evenly;

[0077] (2) placing the system obtained in (1) in a muffle furnace, heating from room temperature to 400° C. at a rate of 2° C. / min in an air atmosphere, and reacting for 120 min;

[0078] (3) The system obtained in (2) is ground to obtain a foamed ZnFe2O4 catalyst (ZnFe2O4-S). Figure 5 are SEM images of different foamy spinel catalysts. Figure 5 It can be seen that the ZnFe2O4 catalyst also has a foamy structure.

[0079] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. Use of a foamed spinel catalyst in the activation of persulfate and the degradation of emerging organic pollutants, characterized in that: The spinel catalyst is: AB2O4, wherein A is a divalent metal and B is a trivalent metal; it has a three-dimensional hierarchical pore structure, including macropores and mesopores, the macropore size is 50-100 nm, and the average mesopore diameter is 3.833 nm; The foamed spinel catalyst is prepared by a method comprising the following steps: S1. Mixing a metal salt precursor and citric acid in a certain proportion; the metal salt precursor is a manganese salt and an iron salt; S2, calcining the system obtained in S1; the calcination temperature is 300-800 ° C, the calcination time is 30-360 min, and the calcination atmosphere is air or pure oxygen; S3. Grind the system obtained in S2 to obtain a foamy spinel catalyst.

2. The use according to claim 1, characterized in that In step S1, the metal salt is at least one of nitrate, sulfate, acetate and chloride.

3. The use according to claim 1, characterized in that In step S1, the molar ratio of citric acid to the metal salt precursor is 0:1-10:

1.

4. The use according to claim 1, characterized in that In step S2, the heating rate is 0.5-10 °C / min.

Citation Information

Patent Citations

  • Application of spinel ferrite catalyst and method for urging persulfate to generate free radicals to catalytically degrade organic matters

    CN103030208A

  • Preparation method of magnetic rare earth barium ferrite nanometer purification catalysts

    CN104998650A

  • Ternary metal oxide catalyst preparation method

    CN107519891A

  • Preparation of spinel catalyst and application thereof to elimination of nitrogen oxides

    CN107790116A

  • Preparation method of nano-scale manganese ferrite catalyst with high specific surface area

    CN109745996A