Reverse-phase rare earth-based ammonia decomposition catalyst and preparation method and application thereof

By using the reverse-phase structure rare earth aminodecomposition catalyst in the catalyst, the rare earth metal is supported on the surface of the active metal particles, increasing interfacial interaction, solving the problem of insufficient activity of the existing catalyst, and significantly improving the ammonia decomposition efficiency and catalytic performance.

CN115920916BActive Publication Date: 2024-11-22TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310041533.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-12
Publication Date
2024-11-22
Estimated Expiration
2043-01-12

AI Technical Summary

Technical Problem

The existing non-precious metal ammonia decomposition catalysts have poor activity, limited active metal content and less metal-support interface content, resulting in low ammonia decomposition efficiency.

Method used

The reverse-phase structure rare earth amidoamino decomposition catalyst is used, and the rare earth metal support is supported on the surface of active metal particles. It is prepared by co-precipitation method to increase the active component content and the metal-support interface, thereby improving the ammonia decomposition efficiency of the catalyst.

Benefits of technology

The efficient conversion of ammonia into hydrogen and nitrogen at high aerial speeds has been achieved, which has significantly improved the hydrogen production efficiency of the catalyst, and has significantly improved the performance of the catalyst prepared by the impregnation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115920916B_ABST
    Figure CN115920916B_ABST
Patent Text Reader

Abstract

The present invention provides a reverse-phase structure rare earth-based ammonia decomposition catalyst and its preparation method and application, the catalyst includes an active metal and a carrier, the active metal is one or two of nickel and cobalt; the carrier is a rare earth metal oxide or a rare earth metal oxide doped with an alkaline earth metal; the mass of the active metal is 10-90wt% of the mass of the rare earth-based ammonia decomposition catalyst. The catalyst is prepared by a coprecipitation method, and an active metal salt, a rare earth metal salt and an alkaline earth metal salt are dissolved in deionized water to obtain a mixed solution; the mixed solution is added dropwise to a sodium hydroxide solution, the precipitation temperature is controlled, and the mixture is stirred, filtered, washed, dried and calcined to obtain. Compared with the supported metal catalyst prepared by the traditional impregnation method, the catalyst of the present invention has a reverse-phase structure, and the rare earth metal oxide is loaded on the surface of the active metal particles, has more active component content and a richer active component-carrier interface, and exhibits excellent catalytic ammonia decomposition hydrogen production activity and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hydrogen production by decomposing ammonia, and in particular to a rare earth-based ammonia decomposition catalyst with an inverse structure, and a preparation method and application thereof. Background Art

[0002] Due to the elemental properties of hydrogen, the storage and transportation technology of pure hydrogen still faces serious bottlenecks. The large-scale use of hydrogen energy faces many challenges. One way to solve this bottleneck is to use hydrogen carriers for transportation and on-site hydrogen production.

[0003] Studies have shown that ammonia, as a chemical hydrogen storage carrier, has the advantages of high thermal efficiency, easy storage and transportation, high safety and no carbon emissions. The biggest advantage of ammonia decomposition hydrogen production compared to other hydrogen production is that the hydrogen produced is zero-carbon hydrogen, which also provides an effective way to solve the hydrogen energy source of fuel cells. The key to developing ammonia decomposition hydrogen production technology is to design ammonia decomposition catalysts with high activity at high space velocity. The ammonia decomposition reaction mainly uses ruthenium precious metal catalysts, but the cost of ruthenium is too high, which limits its practical application. In order to reduce the cost of catalysts, it is more meaningful to develop highly active non-precious metal catalysts, which will promote the development of ammonia decomposition hydrogen production technology and facilitate industrial practical applications. Among non-precious metal catalysts, nickel-based catalysts have higher catalytic activity for ammonia decomposition. Koichi Eguchi's research group used an impregnation method to prepare nickel-based catalysts supported by aluminum oxide, cerium oxide, yttrium oxide and other rare earth metal oxide carriers, and found that the nickel-based catalysts supported by rare earth metal oxides have higher ammonia decomposition activity, which is mainly related to the fact that rare earth metal oxides are conducive to the desorption of hydrogen species. Jiang Lilong's research group used the impregnation method to prepare nickel-based catalysts supported by ceria of different morphologies. Among them, the rod-shaped ceria-supported nickel-based catalyst had the highest ammonia decomposition activity, which was closely related to its smaller nickel particle size. Although a large number of studies have been conducted to improve the catalytic activity of traditional non-precious metal-supported ammonia decomposition catalysts, the limited active metal content and the low metal-support interface content have led to a bottleneck problem in activity. Summary of the invention

[0004] The purpose of the present invention is to provide a rare earth-based ammonia decomposition catalyst with an inverse structure and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art. The structural feature of the inverse structure catalyst is that a rare earth metal carrier is loaded on the surface of active metal particles, has a higher active component content and a richer active component-carrier interface, thereby improving the ammonia decomposition efficiency of the catalyst, realizing efficient conversion of ammonia into hydrogen and nitrogen at high space velocity, and solving the problem of poor activity of non-precious metal ammonia decomposition catalysts.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] The first object of the present invention is to provide a method for preparing a rare earth-based ammonia decomposition catalyst with an inverse structure, wherein the catalyst is a rare earth metal carrier loaded on the surface of an active metal particle, wherein the active metal particle is one or both of nickel and cobalt, and the rare earth metal carrier is a rare earth metal oxide or a rare earth metal oxide doped with an alkaline earth metal, and the mass of the active metal particle is 10% to 90% of the mass of the catalyst. The preparation method comprises the following specific steps:

[0007] S1, dissolving an active metal salt and a carrier metal salt in deionized water, stirring at room temperature for 0.5-8h to obtain a mixed solution, wherein the carrier metal salt is a rare earth metal salt or the carrier metal salt comprises a rare earth metal salt and an alkaline earth metal salt;

[0008] S2, dissolving a certain amount of sodium hydroxide in deionized water, stirring at a certain temperature for 0.5-8h to obtain a sodium hydroxide solution;

[0009] S3, adding the mixed solution obtained in step S1 dropwise to the sodium hydroxide solution obtained in step S2, and continuing stirring at the temperature of step S2 for 1-24 hours, filtering to obtain a precipitate;

[0010] S4, washing the precipitate obtained in step S3 with ethanol and deionized water until the filtrate is neutral, and drying to obtain the reversed rare earth-based ammonia decomposition catalyst; or drying and high-temperature calcining to obtain the reversed rare earth-based ammonia decomposition catalyst.

[0011] Further, when the carrier metal salt is a rare earth metal salt, the active metal salt and the

[0012] dilute

[0013] The mass ratio of the earth metal salt is in the range of (0.05-17.67):1; when the carrier metal salt comprises a rare earth metal salt and an alkaline earth metal salt, the mass ratio of the active metal salt to the rare earth metal salt is (0.22-35.35):1, and the mass ratio of the active metal salt to the alkaline earth metal salt is (5.81-104.64):1.

[0014] Furthermore, in step S1, the active metal salt is any one or two of nickel chloride hexahydrate, nickel sulfate, nickel nitrate hexahydrate, cobalt chloride hexahydrate, cobalt sulfate and cobalt nitrate hexahydrate.

[0015] Further, in step S1, the rare earth metal salt is any one or two of cerium nitrate hexahydrate, lanthanum nitrate hexahydrate, praseodymium nitrate hexahydrate, neodymium nitrate hexahydrate, samarium nitrate hexahydrate, europium nitrate hexahydrate, gadolinium nitrate hexahydrate, terbium nitrate hexahydrate and yttrium nitrate hexahydrate.

[0016] Furthermore, in step S1, the alkaline earth metal salt is any one of magnesium nitrate hexahydrate, barium nitrate, calcium nitrate and strontium nitrate.

[0017] Furthermore, in step S2, the sodium hydroxide solution is heated to a temperature of 20-150°C.

[0018] Furthermore, in step S2, the molar amount of sodium hydroxide is 0.5-10 times the total molar amount of metal.

[0019] Furthermore, in step S3, the high temperature calcination temperature is 300-1000° C., and the calcination time is 0-10 h.

[0020] The second object of the present invention is to provide a rare earth-based ammonia decomposition hydrogen production catalyst with an inverse structure, which is prepared by the above-mentioned preparation method.

[0021] The third object of the present invention is to provide the use of the above-mentioned reverse structure rare earth-based ammonia decomposition hydrogen production catalyst for preparing hydrogen by decomposing ammonia.

[0022] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0023] The catalyst prepared by coprecipitation has a high content of active components. The size of the obtained catalyst metal particles changes with the change of the amount of active components or the temperature of the heated sodium hydroxide solution. The metal particle size ranges from 10 to 20 nm. At a certain content of active metal, the rare earth metal oxide carrier is distributed on the surface of the active component particles and has an inverse structure. The structure of this new inverse catalyst allows the catalyst to form more metal carrier interfaces, has stronger metal carrier interactions, promotes the recombination and desorption of nitrogen, and enhances the hydrogen production efficiency of ammonia decomposition. Compared with conventional supported catalysts prepared by impregnation, the performance of the inverse structure catalyst prepared by coprecipitation is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the structure of samples of Example 1 and Comparative Example 1 of the present invention, a is Comparative Example 1, b is Example 1;

[0025] Figure 2 TEM image of the sample of catalyst example 1 of the present invention;

[0026] Figure 3 This is a comparison chart of the activity test results of samples in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention are further described in detail below in conjunction with specific examples and drawings. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.

[0028] Schematic diagram of the structure of supported metal catalyst prepared by traditional impregnation method Figure 1 As shown in a, the white particles are rare earth metal oxide carriers, and the gray particles are active metal particles. The active metal particles are loaded on the rare earth metal oxide carrier, and the active metal is more distributed on the surface and edge of the carrier;

[0029] The schematic diagram of the structure of the reverse phase rare earth-based ammonia decomposition catalyst of the present invention is as follows Figure 1 As shown in b, the white particles are rare earth metal oxide particles, and the gray particles are active metal particles. Rare earth metal oxide particles are evenly distributed around the active metal particles, and the rare earth metal oxide particles are attached to the active metal particles. The active metal particles and the rare earth metal oxide have more interfaces.

[0030] The active metal salt used in the present invention can be any one or two of nickel chloride hexahydrate, nickel sulfate, nickel nitrate hexahydrate, cobalt chloride hexahydrate, cobalt sulfate and cobalt nitrate hexahydrate. Nickel-based catalysts and cobalt-based catalysts have good ammonia decomposition catalytic performance. The above nickel salts and cobalt salts can form nickel hydroxide or cobalt hydroxide with sodium hydroxide, and form nickel oxide or cobalt oxide after roasting and reduction.

[0031] The rare earth metal salt used in the present invention can be any one or two of cerium nitrate hexahydrate, lanthanum nitrate hexahydrate, praseodymium nitrate hexahydrate, neodymium nitrate hexahydrate, samarium nitrate hexahydrate, europium nitrate hexahydrate, gadolinium nitrate hexahydrate, terbium nitrate hexahydrate and yttrium nitrate hexahydrate. The second rare earth metal doped into a rare earth metal oxide has the function of regulating the interaction between the oxygen vacancies of the catalyst and the metal support, thereby improving the ammonia decomposition performance of the catalyst.

[0032] The alkaline earth metal salt used in the present invention is any one of magnesium nitrate hexahydrate, barium nitrate, calcium nitrate and strontium nitrate. The doping of alkaline earth metal can regulate the electron distribution or enhance the metal-carrier interaction.

[0033] Example 1

[0034] Weigh 5.46 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 1.85 grams of cerium nitrate hexahydrate and stir for 0.5 hours after complete dissolution to obtain a mixed solution; weigh 2.01 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (60wt% Ni-CeO2) with a nickel metal content of 60wt%.

[0035] like Figure 2 As shown, it is a transmission electron microscope image (TEM image) of the 60wt% Ni-CeO2 catalyst prepared in this embodiment. In the figure, the solid line is the active metal nickel particles, and the dotted line is the rare earth metal oxide cerium dioxide particles. Obviously, the nickel particles and the cerium dioxide particles form a more obvious interface.

[0036] Example 2

[0037] 5.46 g of nickel nitrate hexahydrate was dissolved in 25 ml of water, and stirred to completely dissolve. Then, 2.49 g of yttrium nitrate hexahydrate was added, and stirred for 0.5 h after complete dissolution to obtain a mixed solution. 2.28 g of sodium hydroxide was dissolved in 25 ml of water, and stirred to completely dissolve, and stirred in an oil bath at 80° C. for 0.5 h. The mixed solution was added dropwise into the sodium hydroxide solution, and stirred for 2 h. The mixture was filtered, and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 400° C. for 2 h, an yttrium oxide-nickel catalyst (60wt% Ni-Y2O3) with a nickel metal content of 60wt% was obtained.

[0038] Example 3

[0039] 5.46 g of nickel nitrate hexahydrate was dissolved in 25 ml of water, and stirred to completely dissolve. Then, 1.87 g of samarium nitrate hexahydrate was added, and stirred for 0.5 h after complete dissolution to obtain a mixed solution. 2.01 g of sodium hydroxide was dissolved in 25 ml of water, and stirred to completely dissolve, and stirred in an oil bath at 80° C. for 0.5 h. The mixed solution was added dropwise into the sodium hydroxide solution, and stirred for 2 h. The mixture was filtered, and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 400° C. for 2 h, a samarium oxide-nickel catalyst (60wt% Ni-Sm2O3) with a nickel metal content of 60wt% was obtained.

[0040] Example 4

[0041] 5.46 g of nickel nitrate hexahydrate was weighed and dissolved in 25 ml of water, and stirred to completely dissolve. Then, 1.85 g of cerium nitrate hexahydrate was added, and stirred for 0.5 h after complete dissolution to obtain a mixed solution; 3.02 g of sodium hydroxide was weighed and dissolved in 25 ml of water, and stirred to completely dissolve, and stirred in an oil bath at 80° C. for 0.5 h; the mixed solution was added dropwise into the sodium hydroxide solution and stirred for 2 h; the filtrate was filtered, and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 400° C. for 2 h, a cerium oxide-nickel (excess sodium hydroxide) catalyst (60wt% Ni-CeO2-1.5NaOH) with a nickel metal content of 60wt% was obtained.

[0042] Example 5

[0043] Weigh 8.19 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 0.46 grams of cerium nitrate hexahydrate, and stir for 0.5 hours after completely dissolving to obtain a mixed solution; weigh 2.38 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (90wt% Ni-CeO2) with a nickel metal content of 90wt%.

[0044] Example 6

[0045] Weigh 7.28 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 0.93 grams of cerium nitrate hexahydrate, and stir for 0.5 hours after complete dissolution to obtain a mixed solution; weigh 2.26 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (80wt% Ni-CeO2) with a nickel metal content of 80wt%.

[0046] Example 7

[0047] Weigh 6.37 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 1.39 grams of cerium nitrate hexahydrate and stir for 0.5 hours to obtain a mixed solution; weigh 2.14 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (70wt% Ni-CeO2) with a nickel metal content of 70wt%.

[0048] Example 8

[0049] Weigh 4.55 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 2.32 grams of cerium nitrate hexahydrate and stir for 0.5 hours to obtain a mixed solution; weigh 1.89 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (50wt% Ni-CeO2) with a nickel metal content of 50wt%.

[0050] Example 9

[0051] Weigh 3.64 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 2.78 grams of cerium nitrate hexahydrate and stir for 0.5 hours to obtain a mixed solution; weigh 1.77 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (40wt% Ni-CeO2) with a nickel metal content of 40wt%.

[0052] Example 10

[0053] Weigh 2.73 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 3.24 grams of cerium nitrate hexahydrate and stir for 0.5 hours to obtain a mixed solution; weigh 1.65 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (30wt% Ni-CeO2) with a nickel metal content of 30wt%.

[0054] Embodiment 11

[0055] Weigh 0.91 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 4.17 grams of cerium nitrate hexahydrate and stir for 0.5 hours to obtain a mixed solution; weigh 1.40 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel catalyst (10wt% Ni-CeO2) with a nickel metal content of 10wt%.

[0056] Example 12

[0057] 5.46 g of nickel nitrate hexahydrate was weighed and dissolved in 25 ml of water. After stirring to completely dissolve, 1.62 g of cerium nitrate hexahydrate was added. After stirring to completely dissolve, 0.16 g of barium nitrate was added. After completely dissolving, it was stirred for 0.5 h to obtain a mixed solution; 2.00 g of sodium hydroxide was weighed and dissolved in 25 ml of water. After stirring to completely dissolve, it was stirred in an oil bath at 80° C. for 0.5 h; the mixed solution was added dropwise into the sodium hydroxide solution and stirred for 2 h; the filtrate was filtered, washed with ethanol and deionized water until the filtrate was neutral, and after complete drying and calcination at 400° C. for 2 h, a cerium oxide-barium oxide-nickel catalyst (60wt% Ni-5wt% BaO-CeO2) with a nickel metal content of 60wt% and a barium oxide content of 5wt% was obtained.

[0058] Embodiment 13

[0059] 5.46 g of nickel nitrate hexahydrate was weighed and dissolved in 25 ml of water. After stirring to completely dissolve, 1.62 g of cerium nitrate hexahydrate was added. After stirring to completely dissolve, 0.19 g of strontium nitrate was added. After completely dissolving, the mixture was stirred for 0.5 h to obtain a mixed solution. 2.02 g of sodium hydroxide was weighed and dissolved in 25 ml of water. After stirring to completely dissolve, the mixture was stirred in an oil bath at 80° C. for 0.5 h. The mixed solution was added dropwise into the sodium hydroxide solution and stirred for 2 h. The mixture was filtered and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 400° C. for 2 h, a cerium oxide-strontium oxide-nickel catalyst (60wt% Ni-5wt% SrO-CeO2) with a nickel metal content of 60wt% and a strontium oxide content of 5wt% was obtained.

[0060] Embodiment 14

[0061] 5.46 g of nickel nitrate hexahydrate was weighed and dissolved in 25 ml of water, and after stirring, it was completely dissolved. Then, 1.62 g of cerium nitrate hexahydrate was added, and after stirring, it was completely dissolved. Then, 0.58 g of magnesium nitrate hexahydrate was added, and after it was completely dissolved, it was stirred for 0.5 h to obtain a mixed solution; 2.13 g of sodium hydroxide was weighed and dissolved in 25 ml of water, and after stirring, it was completely dissolved, it was stirred in an oil bath at 80° C. for 0.5 h; the mixed solution was added dropwise into the sodium hydroxide solution, and stirred for 2 h; the filtrate was filtered, and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 400° C. for 2 h, a cerium oxide-magnesium oxide-nickel catalyst (60wt% Ni-5wt% MgO-CeO2) with a nickel metal content of 60wt% and a magnesium oxide content of 5wt% was obtained.

[0062] Embodiment 15

[0063] Weigh 3.63 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 1.82 grams of cobalt nitrate hexahydrate and stir to completely dissolve it. Then add 1.85 grams of cerium nitrate hexahydrate and stir for 0.5 hours after it is completely dissolved to obtain a mixed solution; weigh 2.01 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve it, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying and calcination at 400°C for 2 hours, obtain a cerium oxide-nickel cobalt catalyst (60wt% Ni2Co-CeO2) with a total nickel and cobalt metal content of 60wt%.

[0064] Example 16

[0065] 5.46 g of nickel nitrate hexahydrate was dissolved in 25 ml of water, and stirred to completely dissolve. Then, 1.85 g of cerium nitrate hexahydrate was added, and stirred for 0.5 h after complete dissolution to obtain a mixed solution. 2.01 g of sodium hydroxide was dissolved in 25 ml of water, and stirred to completely dissolve, and stirred in an oil bath at 60° C. for 0.5 h. The mixed solution was added dropwise into the sodium hydroxide solution, and stirred for 2 h. The mixture was filtered, and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 400° C. for 2 h, a cerium oxide-nickel catalyst (60wt% Ni-CeO2-60° C.) with a nickel metal content of 60wt% was obtained.

[0066] Embodiment 17

[0067] 5.46 g of nickel nitrate hexahydrate was dissolved in 25 ml of water, and stirred to completely dissolve. Then, 1.85 g of cerium nitrate hexahydrate was added, and stirred for 0.5 h after complete dissolution to obtain a mixed solution. 2.01 g of sodium hydroxide was dissolved in 25 ml of water, and stirred to completely dissolve, and stirred in an oil bath at 100° C. for 0.5 h. The mixed solution was added dropwise into the sodium hydroxide solution, and stirred for 2 h. The filtrate was filtered, and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 400° C. for 2 h, a cerium oxide-nickel catalyst (60wt% Ni-CeO2-100° C.) with a nickel metal content of 60wt% was obtained.

[0068] Embodiment 18

[0069] Weigh 5.46 grams of nickel nitrate hexahydrate and dissolve it in 25 ml of water. After stirring to completely dissolve, add 1.85 grams of cerium nitrate hexahydrate and stir for 0.5 hours after complete dissolution to obtain a mixed solution; weigh 2.01 grams of sodium hydroxide and dissolve it in 25 ml of water. After stirring to completely dissolve, stir in an oil bath at 80°C for 0.5 hours; add the mixed solution drop by drop into the sodium hydroxide solution and stir for 2 hours; filter with suction, wash with ethanol and deionized water until the filtrate is neutral, and after complete drying, obtain a cerium oxide-nickel catalyst (60wt% Ni-CeO2CP) with a nickel metal content of 60wt%.

[0070] Embodiment 19

[0071] 5.46 g of nickel nitrate hexahydrate was dissolved in 25 ml of water, and stirred to completely dissolve. Then, 1.85 g of cerium nitrate hexahydrate was added, and stirred for 0.5 h after complete dissolution to obtain a mixed solution. 2.01 g of sodium hydroxide was dissolved in 25 ml of water, and stirred to completely dissolve, and stirred in an oil bath at 80°C for 0.5 h. The mixed solution was added dropwise into the sodium hydroxide solution, and stirred for 2 h. The filtrate was filtered, and washed with ethanol and deionized water until the filtrate was neutral. After complete drying and calcination at 600°C for 2 h, a cerium oxide-nickel catalyst (600°C-60wt% Ni-CeO2) with a nickel metal content of 60 wt% was obtained.

[0072] Embodiment 20

[0073] 5.46 g of nickel nitrate hexahydrate was dissolved in 25 ml of water, and stirred to completely dissolve. Then, 1.85 g of cerium nitrate hexahydrate was added, and stirred for 0.5 h after complete dissolution to obtain a mixed solution. 2.01 g of sodium hydroxide was dissolved in 25 ml of water, and stirred to completely dissolve, and stirred in an oil bath at 80°C for 0.5 h. The mixed solution was added dropwise into the sodium hydroxide solution, and stirred for 2 h. Filtered, washed with ethanol and deionized water until the filtrate was neutral, and after complete drying and calcination at 800°C for 2 h, a cerium oxide-nickel catalyst (800°C-60wt% Ni-CeO2) with a nickel metal content of 60 wt% was obtained.

[0074] Comparative Example 1

[0075] 0.50 g of nickel nitrate hexahydrate was dissolved in 1.50 g of aqueous solution as the impregnation solution, 0.90 g of cerium dioxide was weighed as the catalyst carrier, the impregnation solution was impregnated onto the cerium dioxide carrier by the impregnation method, and dried at 80°C overnight, and finally calcined at 600°C for 2 h to obtain a cerium oxide-nickel impregnation catalyst (10wt% Ni / CeO2) with a nickel loading of 10wt%.

[0076] In order to better illustrate the catalytic hydrogen production effect of the reverse-phase rare earth-based ammonia decomposition catalyst of the present invention, the catalyst reaction performance evaluation was carried out.

[0077] The ammonia decomposition performance of the ammonia decomposition catalyst prepared in Examples 1-17 was tested and evaluated in an ammonia decomposition fixed bed reactor. The fixed bed reactor quartz tube has an inner diameter of 6 mm and an outer diameter of 8 mm. 0.1-0.2 g of catalyst (20-40 mesh) was mixed with 0.8 g of quartz sand and reduced at 400°C for 2 h under the condition of 30 ml / min hydrogen and then heated to 600°C at 10°C / min. The flow rate of ammonia during the test was 50 ml / min, and the reaction space velocity was 30000 mL·h -1 ·g cat -1 The reaction temperatures are 450°C, 500°C, 550°C and 600°C. The catalyst activity results are shown in Table 1.

[0078] It can be seen from Table 1 that the ammonia decomposition catalysts prepared in Examples 1-20 of the present invention have higher activity than the 10 wt % Ni / CeO 2 catalyst in Comparative Example 1.

[0079] Table 1.

[0080]

[0081] like Figure 3 As shown, the activity test comparison chart of the samples of Example 1 of the present invention and Comparative Example 1. Figure 3 It can be seen that the ammonia decomposition rate of the sample in Example 1 is relatively high; at 350-600°C, 30000 mL·h -1 ·g cat -1 The higher the space velocity, the higher the activity.

[0082] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a rare earth-based ammonia decomposition catalyst with an inverse structure, characterized in that: The catalyst is a rare earth metal carrier loaded on the surface of an active metal particle, the active metal particle is one or both of nickel and cobalt, the rare earth metal carrier is a rare earth metal oxide or a rare earth metal oxide doped with an alkaline earth metal, the mass of the active metal particle is 10% to 90% of the mass of the catalyst, and the preparation method comprises the following specific steps: S1, dissolving an active metal salt and a carrier metal salt in deionized water, stirring at room temperature for 0.5-8h to obtain a mixed solution, wherein the carrier metal salt is a rare earth metal salt or the carrier metal salt comprises a rare earth metal salt and an alkaline earth metal salt; When the carrier metal salt is a rare earth metal salt, the mass ratio of the active metal salt to the rare earth metal salt is in the range of (0.05-17.67):1; when the carrier metal salt comprises a rare earth metal salt and an alkaline earth metal salt, the mass ratio of the active metal salt to the rare earth metal salt is in the range of (0.22-35.35):1, and the mass ratio of the active metal salt to the alkaline earth metal salt is in the range of (5.81-104.64):1; The active metal salt is any one or two of nickel chloride hexahydrate, nickel sulfate, nickel nitrate hexahydrate, cobalt chloride hexahydrate, cobalt sulfate and cobalt nitrate hexahydrate; The rare earth metal salt is any one or two of cerium nitrate hexahydrate, lanthanum nitrate hexahydrate, praseodymium nitrate hexahydrate, neodymium nitrate hexahydrate, samarium nitrate hexahydrate, europium nitrate hexahydrate, gadolinium nitrate hexahydrate, terbium nitrate hexahydrate and yttrium nitrate hexahydrate; The alkaline earth metal salt is any one of magnesium nitrate hexahydrate, barium nitrate, calcium nitrate and strontium nitrate; S2, dissolving a certain amount of sodium hydroxide in deionized water, stirring at a certain temperature for 0.5-8h to obtain a sodium hydroxide solution; S3, adding the mixed solution obtained in step S1 dropwise to the sodium hydroxide solution obtained in step S2, and continuing stirring at the temperature of step S2 for 1-24 hours, filtering to obtain a precipitate; S4, washing the precipitate obtained in step S3 with ethanol and deionized water until the filtrate is neutral, and drying to obtain the reversed rare earth-based ammonia decomposition catalyst; or drying and high-temperature calcining to obtain the reversed rare earth-based ammonia decomposition catalyst.

2. The preparation method according to claim 1, characterized in that In step S2, the sodium hydroxide solution is heated to a temperature of 20-150°C.

3. The preparation method according to claim 2, characterized in that: In step S2, the molar amount of sodium hydroxide is 0.5-10 times the total molar amount of metal.

4. The preparation method according to claim 3, characterized in that: In step S3, the high temperature calcination temperature is 300-1000° C., and the calcination time is 0-10 h.

5. A rare earth-based catalyst for hydrogen production by decomposition of ammonia with an inverse structure, characterized in that: The method is prepared according to any one of claims 1 to 4.

6. The use of the reverse-phase rare earth-based ammonia decomposition hydrogen production catalyst as claimed in claim 5, characterized in that: The catalyst is used for decomposing ammonia to produce hydrogen.