High elasticity and high sealing porous carbon block material and preparation method thereof

By using amorphous carbon-coated porous carbon bulk materials with diamond nanoparticles and using high-pressure and high-temperature sintering technology, the problems of insufficient elastic deformation ability and open pores of inorganic materials are solved, achieving high strength, high air tightness and low density porous materials. Carbon material, suitable for sealing applications in complex environments.

CN115925420BActive Publication Date: 2024-10-01YANSHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111168176.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-30
Publication Date
2024-10-01
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

Existing inorganic non-metallic materials have limited elastic deformation capabilities at room temperature, and the open pores of porous carbon materials result in insufficient compressive strength, which limits their application scope.

Method used

Amorphous carbon-coated diamond nanoparticles are used to prepare porous carbon bulk materials through discharge plasma sintering or hot pressing methods to form a closed-pore structure with a pore diameter of 3-100nm and a porosity of 50-87%, combined with high-pressure and high-temperature sintering technology.

Benefits of technology

A porous carbon material with high strength, high elasticity and high air tightness has been achieved, with compressive strain ≥5%, compressive strength >100MPa, and extremely low helium leakage rate, making it suitable for sealing materials in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115925420B_ABST
    Figure CN115925420B_ABST
Patent Text Reader

Abstract

The present application provides a porous carbon block material with high elasticity and high sealing performance and a preparation method thereof. Specifically, the present application provides a porous carbon block material, wherein the pore size range of the porous carbon block material is 3-100nm, the porosity is 50-87%, and the pores in the porous carbon block material are closed pores. The present application also provides a method for preparing the porous carbon block material of the present application. The porous carbon block material of the present application has a small pore size, high porosity, and all pores are closed pores, so it has high strength and high elasticity at the same time, and has high sealing performance and low density, and can be used as a sealing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon material preparation, and in particular to a porous carbon block material and a method for preparing the porous carbon block material. Background Art

[0002] Inorganic non-metallic materials are usually brittle and can only show very small elastic deformation (usually less than 1%) at room temperature. When their elastic limit is exceeded, the microcracks in the material will expand rapidly, resulting in instantaneous destruction of the material. The extremely poor deformation ability severely limits the application scope of inorganic non-metallic materials. In modern material design, designing and manufacturing high-performance inorganic non-metallic materials with high strength, high elasticity and low density is a long-term goal and challenge.

[0003] Since carbon has the ability to form sp, sp 2 、sp 3 The flexibility of hybrid bonds may therefore become materials with excellent comprehensive properties, such as low density, high strength, high hardness, high elasticity, and adjustable electronic properties. Generally speaking, low-density and high-elasticity carbon materials can be obtained by constructing porous structures. For example, the recently developed carbon-based porous materials have the advantages of both low density and excellent elastic deformation ability. However, the pores of these known porous materials are open and not airtight, and the compressive strength generally does not exceed 1MPa, which limits their scope of application. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a carbon material having high strength, high elasticity, high sealing and low density, and the carbon material of the present invention can adapt to various complex environments.

[0005] In one aspect, the present invention provides a porous carbon block material, wherein:

[0006] The pore size of the porous carbon block material is in the range of 3-100 nm;

[0007] The porosity of the porous carbon block material is 50-87%; and

[0008] The pores in the porous carbon block material are closed pores.

[0009] The porous carbon block material of the present invention can be synthesized by spark plasma sintering or hot pressing, for example, using amorphous carbon-coated diamond nanoparticles as initial raw materials.

[0010] In one embodiment of the porous carbon block material of the present invention, the pore size range of the porous carbon block material is 3-100nm (for example, 4-100nm or 5-100nm); preferably, the pore size range of the porous carbon block material is 5-70nm or 5-50nm; more preferably, the pore size range of the porous carbon block material is 5-40nm or 5-30nm.

[0011] In one embodiment of the porous carbon block material of the present invention, the porosity of the porous carbon block material is 50-87%; preferably, the porosity of the porous carbon block material is 56-82%; more preferably, the porosity of the porous carbon block material is 60-80%.

[0012] In a preferred embodiment of the porous carbon block material of the present invention, the grain size of the amorphous carbon-coated diamond nanoparticles is 5-400nm; preferably, the grain size of the amorphous carbon-coated diamond nanoparticles is preferably 5-350nm; more preferably, the grain size of the amorphous carbon-coated diamond nanoparticles is 5-300nm.

[0013] In a preferred embodiment of the porous carbon block material of the present invention, the compressive strain of the porous carbon block material is ≥5%; more preferably, the compressive strain of the porous carbon block material is ≥6%; most preferably, the compressive strain of the porous carbon block material is ≥7%. In addition, in a preferred embodiment of the porous carbon block material of the present invention, the compressive strain of the porous carbon block material returns to zero after the stress is removed.

[0014] In a preferred embodiment of the porous carbon block material of the present invention, the compressive strength of the porous carbon block material is greater than 100 MPa, and more preferably, the compressive strength of the porous carbon block material is greater than 150 MPa.

[0015] In a preferred embodiment of the porous carbon block material of the present invention, the helium leakage rate of the porous carbon block material is ≤10×10 -5 Pa·m 3 / s; More preferably, the helium leakage rate of the porous carbon block material is ≤4×10 -5 Pa·m 3 / s; Most preferably, the helium leakage rate of the porous carbon block material is ≤2×10 -5 Pa·m 3 / s.

[0016] In a preferred embodiment of the porous carbon block material of the present invention, the density of the porous carbon block material is 0.3-1.1 g / cm 3 More preferably, the density of the porous carbon block material is 0.4-1.0 g / cm 3Most preferably, the density of the porous carbon block material is 0.5-0.9 g / cm 3 .

[0017] In an embodiment of the porous carbon block material of the present invention, the porous material is synthesized by spark plasma sintering or hot pressing using amorphous carbon-coated diamond nanoparticles as initial raw materials. Preferably, the initial raw materials of the porous material are only amorphous carbon-coated diamond nanoparticles. In this article, amorphous carbon-coated diamond nanoparticles are materials known in the art. In a preferred embodiment of the porous carbon block material of the present invention, the grain size of the amorphous carbon-coated diamond nanoparticles is 5-400nm, preferably 5-350nm, and more preferably 5-300nm.

[0018] In another aspect, the present invention provides a method for preparing the porous carbon block material according to the first aspect of the present invention, comprising:

[0019] A) Amorphous carbon-coated diamond nanoparticles as precursor powder;

[0020] B) placing the precursor powder of step A) into a mold and pre-pressing to obtain a pre-pressed green body;

[0021] C) placing the pre-pressed green body obtained in step B) into a sintering mold, and then placing the sintering mold containing the pre-pressed green body into a sintering device, applying sintering pressure, and then heating to a sintering temperature, maintaining the temperature, and sintering, wherein:

[0022] The sintering pressure is 5-100MPa,

[0023] The sintering temperature is 1000-2000℃;

[0024] D) Take out the mold, demould, and obtain a porous carbon block material.

[0025] In an embodiment of the inventive method, the raw material used may be amorphous carbon coated diamond nanoparticles. Preferably, the raw material used is only amorphous carbon coated diamond nanoparticles. In this article, amorphous carbon coated diamond nanoparticles are materials known in the art. In a preferred embodiment of the inventive method, the grain size of the amorphous carbon coated diamond nanoparticles of step A) is 5-400nm, preferably 5-350nm, more preferably 5-300nm.

[0026] In a preferred embodiment of the method of the present invention, the pre-pressing in step B) is performed by applying pressure in both directions, and the applied pressure is 1-20 MPa, preferably 2-15 MPa, more preferably 2-10 MPa, and most preferably 2-5 MPa.

[0027] In a similarly preferred embodiment of the method of the present invention, the holding time of the pre-pressing in step B) is 1-20 min, preferably 1-15 min, more preferably 1-10 min, and most preferably 1-5 min.

[0028] In a preferred embodiment of the method of the present invention, the sintering pressure in step C) is 5-100 MPa, preferably 5-80 MPa, more preferably 10-70 MPa.

[0029] In a preferred embodiment of the method of the present invention, the sintering temperature in step C) is 1000-2000°C, preferably 1300-2000°C, more preferably 1400-2000°C.

[0030] In a preferred embodiment of the method of the present invention, the heating rate in step C) is 5-200° C. / min, preferably 8-150° C. / min, more preferably 10-100° C. / min.

[0031] In a preferred embodiment of the method of the present invention, the holding time in step C) is 0-30 min, preferably 0-20 min, more preferably 0-15 min.

[0032] In a preferred embodiment of the method of the present invention, the sintering mold in step C) is a graphite mold, wherein the pre-pressed body and the graphite mold are separated by graphite paper, and the periphery of the graphite mold is wrapped with carbon felt.

[0033] In a preferred embodiment of the method of the present invention, the sintering in step C) is spark plasma sintering or hot pressing sintering.

[0034] In a preferred embodiment of the method of the present invention, in step C), before applying the sintering pressure, an initial pressure of 2-10 MPa is optionally applied, and the vacuum is evacuated to a vacuum degree of more than 1×10 -1 Pa, and then apply sintering pressure.

[0035] In a preferred embodiment of the method of the present invention, in step C), after the sintering pressure is stabilized at a preset value, the temperature is raised to the sintering temperature, the temperature is maintained, and sintering is performed.

[0036] Preferably, after sintering is completed and before step D), step C') is included: after sintering is completed, cooling and decompression to normal pressure, preferably, the cooling rate is 100-1000° C. / min.

[0037] The porous carbon block material described in the first aspect of the present invention and the porous carbon block material prepared by the method described in the second aspect of the present invention have small pore size, high porosity and are closed pores, and thus, have high strength and high elasticity, high air tightness and low density. In particular, the porous carbon block material described in the first aspect of the present invention and the porous carbon block material prepared by the method described in the second aspect of the present invention can be used as a sealing material due to its high elasticity and good air tightness. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The skilled person will understand that the drawings described below are for illustration purposes only. These drawings are not intended to limit the scope of the present invention in any way.

[0039] Figure 1 (a) is a physical picture of a porous carbon block material prepared according to one embodiment of the present invention; Figure 1 (b) is a photograph of a porous carbon block material prepared according to one embodiment of the present invention floating in water.

[0040] Figure 2 These are the X-ray diffraction patterns of the porous carbon block materials obtained in Examples 1-3 of the present invention, wherein (a) is Example 1, (b) is Example 2, and (c) is Example 3.

[0041] Figure 3 This is a high-resolution transmission electron microscopic image of the porous carbon block material prepared in Example 1 of the present invention.

[0042] Figure 4 This is a bright field transmission electron microscopic image of the porous carbon block material prepared in Example 1 of the present invention.

[0043] Figure 5 is a scanning electron microscope image of a porous carbon bulk material prepared according to one embodiment of the present invention.

[0044] Figure 6 The uniaxial compression stress-strain curves of the porous carbon block materials prepared in Examples 1-3 of the present invention at room temperature, wherein (a) is Example 1, (b) is Example 2, and (c) is Example 3.

[0045] Figure 7 The room temperature cyclic compression stress-strain curves of the porous carbon block materials prepared in Examples 1-3 of the present invention, wherein (a) is Example 1, (b) is Example 2, and (c) is Example 3;

[0046] Figure 8 This is the cyclic compression stress-strain curve of the porous carbon block material obtained in Example 1 of the present invention measured at 600° C. in an air atmosphere.

[0047] Fig. 9 It is a schematic diagram of a helium leak rate test device.

[0048] Fig.10 yes Fig. 9 A partial enlarged view of component 3 in the helium leakage rate test device. DETAILED DESCRIPTION

[0049] Herein, when a material is described as containing, comprising, or including specific components, or when a method is described as containing, comprising, or including specific steps, it is intended that the material of the present invention consists essentially of or consists of the specific components, and the method of the present invention consists essentially of or consists of the specific steps.

[0050] Unless expressly stated otherwise, the terms "including," "comprising," "containing," and "having" are to be construed as open ended and non-limiting.

[0051] Unless otherwise expressly stated, the method steps and other operations of the present invention are carried out at normal temperature and pressure.

[0052] Where a numerical range is disclosed herein, this numerical range is continuous and includes the minimum and maximum values ​​of the range and each value between the minimum and maximum values. In addition, where a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, where multiple ranges are provided to describe features or characteristics, these ranges can be combined. That is, unless otherwise indicated, all ranges disclosed herein are to be understood to encompass any and all sub-ranges contained therein. For example, the specified range of "1-10" is to be deemed to include any and all sub-ranges between the minimum value 1 and the maximum value 10. In addition, the amount range of each component of the present invention includes any combination of any lower limit and any upper limit mentioned in the specification, and all these ranges are encompassed within the scope of the present invention.

[0053] When used herein, as understood by those skilled in the art, "about" means that in the specific scientific context of the term, the number, parameter or feature defined by it allows positive and negative percentage errors within a certain range (e.g., ±5%). In addition, since all numbers, values ​​and expressions related to the amounts used herein are subject to various measurement errors, unless otherwise specified, all recorded specific values ​​can be understood as implicitly modified by the term "about".

[0054] In this article, preferred ranges of values ​​for certain performances or parameters in preferred embodiments are also provided. It will be appreciated by those skilled in the art that the respective ranges of values ​​for the different performance parameters in these different embodiments can be combined in any manner, and all possible combinations are considered to be disclosed in this article.

[0055] According to a first aspect of the present invention, there is provided a porous carbon block material made of diamond nanoparticles coated with amorphous carbon, wherein:

[0056] The pore size of the porous carbon block material is in the range of 3-100 nm;

[0057] The porosity of the porous carbon block material is 60-80%; and

[0058] The pores in the porous carbon block material are closed pores.

[0059] In this context, "bulk material" means that the material is a solid mass with a certain volume, that is, a solid material that does not exist in the form of granular material or powder material.

[0060] The porous carbon block material of the present invention has a small pore size. In a preferred embodiment of the porous carbon block material of the present invention, the pore size range of the porous carbon block material may be 3-100 nm, preferably 5-50 nm, and more preferably 5-30 nm. Herein, the pore size of the porous carbon block material can be directly measured by a high-resolution transmission electron microscopy image. Herein, the "pore size range of ab nm" of the material means that when the pore size of the material is measured by, for example, a high-resolution transmission electron microscopy image, the pore size of the vast majority of pores in the material falls within the range of a nm to b nm. Those skilled in the art will understand that, due to the limitations of the material manufacturing process, the "pore size range of ab nm" of the material does not exclude the situation where the pore size of a small number of pores falls outside the range of a nm to b nm. Therefore, "pore size range of ab nm" means that at least 80%, for example at least 90%, preferably at least 95%, and most preferably at least 98% of the pores, in terms of the number of pores, have a pore size that falls within the range of a nm to b nm. For example, one or more (eg, 3, 5, or 10) randomly selected regions of the material may be observed using a transmission electron microscope, and the pore sizes in the regions may be statistically analyzed to determine the percentage of pore sizes within a specified range.

[0061] The porous carbon block material of the present invention has a high porosity. In a preferred embodiment of the porous carbon block material of the present invention, the porosity of the porous carbon block material may be 50-87%, preferably 56-82%, and more preferably 60-80%. Herein, the porosity of the porous carbon block material is calculated based on the density of the sample obtained by the test and the theoretical density of graphite. Specifically, the porosity calculation method is as follows:

[0062] k=1-ρ 样品 / ρ 石墨 ,

[0063] Where k is the porosity, ρ 样品 is the density of the sample, ρ 石墨is the theoretical density of graphite (2.26 g / cm 3 ).

[0064] The measurement and calculation methods of sample density are described below.

[0065] The pores in the porous carbon block material of the present invention are closed pores. Through transmission electron microscopy observation, the curved multi-layer graphene sheets after sintering are arranged chaotically, and the curved graphene is cross-linked and supported to form a large number of closed nanoscale holes. In this article, "the pores in the material are closed pores" means that when observed by, for example, a transmission electron microscope, the vast majority of the pores in the material are closed pores. It can be understood by those skilled in the art that due to the limitations of the material manufacturing process, "the pores in the material are closed pores" does not exclude the situation where a small number or individual pores are open pores. Therefore, "the pores in the material are closed pores" means that at least 90%, such as 95%, preferably at least 96%, and most preferably at least 98% of the pores are closed pores in terms of the number of pores. For example, one or more (for example, 3, 5 or 10) areas of a randomly selected material can be observed using a transmission electron microscope, and the pores in the area can be analyzed and statistically determined to determine the percentage of closed pores.

[0066] Scanning electron microscopy observation shows that the cross section of the porous carbon block material of the present invention is flat, and substantially no micron-sized pores are present therein (eg, the number of micron-sized pores is less than 3‰, more preferably less than 1‰).

[0067] In this paper, the porous carbon block material is made of amorphous carbon-coated diamond nanoparticles. The use of amorphous carbon-coated diamond nanoparticles, on the one hand, amorphous carbon-coated diamond is a metastable phase, and graphitization structure transformation will occur during the sintering process, accompanied by volume expansion, which is conducive to the bonding between particles and improves the block strength; on the other hand, the surface activity of amorphous carbon-coated diamond powder is high, and it quickly graphitizes during the sintering process to form high-curvature graphene sheets. These graphene sheets are cross-linked and supported with each other, which is easy to form pores and reduce the density of the material. Moreover, the onion-like graphene layer transformed from the small-particle diamond phase has a higher curvature, which is easier to form evenly distributed voids, and is also more likely to undergo interlayer cross-linking, forming a stable connection between graphene sheets, and is more likely to undergo elastic deformation under the action of external forces, but not easy to be damaged, thereby improving the elastic limit of the sample. In a preferred embodiment of the porous carbon block material of the present invention, the amorphous carbon-coated diamond nanoparticles have a grain size of 5-400 nm, preferably 5-350 nm, and more preferably 5-300 nm.

[0068] In a preferred embodiment of the porous carbon block material of the present invention, the density of the porous carbon block material is 0.3-1.1 g / cm 3, preferably 0.4-1.0g / cm 3 , more preferably 0.5-0.9 g / cm 3 In particular, the density of the porous carbon block material of the present invention is preferably not higher than 0.7 g / cm 3 , for example 0.5-0.7 g / cm 3 .

[0069] In this paper, the density of the porous carbon block material is obtained by dividing the sample mass by the volume. First, the sample is processed into a cylinder with a diameter of 20 mm and a height of 5 mm, and the volume sample volume V is calculated according to the cylinder volume calculation formula 样品 , and then use a high-precision electronic balance to test the sample mass m 样品 . Sample density ρ 样品 =m 样品 / V 样品 .

[0070] In a preferred embodiment of the porous carbon block material of the present invention, the compressive strain of the porous carbon block material is ≥5%; preferably, the compressive strain of the porous carbon block material is ≥6%; more preferably, the compressive strain is ≥7%.

[0071] In a preferred embodiment of the porous carbon block material of the present invention, the compressive strength of the porous carbon block material is >100MPa, preferably >150MPa. For example, the compressive strength of the porous carbon block material of the present invention may be 100-400MPa, preferably 120-350MPa, and more preferably 150-300MPa.

[0072] In this article, the compressive strain and compressive strength of the porous carbon block material are measured according to the method described in GB / T 8489-2006. The measurement of compressive strength and compressive strain can be carried out on a conventional material mechanical properties testing machine in the art, and various performance tests are carried out on the test sample at room temperature. The test sample can be a cylinder, and the test sample size is, for example, 3 mm in diameter and 4.5 mm in height. The loading strain rate of the material mechanical properties testing machine is, for example, 1×10 -5 -1×10 -2 The material mechanical properties testing machine used in the present invention is, for example, a TE-3000 mechanical testing machine produced by Jinan Jinyinfeng Instrument Co., Ltd.

[0073] In a preferred embodiment of the porous carbon block material of the present invention, the helium leakage rate of the porous carbon block material is ≤10×10 -5 Pa·m 3 / s; preferably, the helium leakage rate of the porous carbon block material of the present invention is ≤5×10 -5 Pa·m 3 / s; More preferably, the helium leakage rate of the porous carbon block material of the present invention is ≤2×10-5 Pa·m 3 / s. For example, the helium leakage rate of the porous carbon block material of the present invention can be 0.2×10 -5 -10×10 -5 Pa·m 3 / s, preferably 1×10 -5 -5×10 -5 Pa·m 3 / s, more preferably 1×10 -5 -2×10 -5 Pa·m 3 / s, and can even reach 0.2×10 -5 -1×10 -5 Pa·m 3 / s.

[0074] In this paper, the sealing of the sample is characterized by testing its helium leakage rate. Helium is one of the smallest gas molecules and can quickly penetrate small leaks. It is chemically inert, does not react with any material in the tested part, and only exists in trace amounts (5ppm) in the atmosphere. Using helium leakage rate to characterize the airtightness of devices and components has become a high-precision airtightness test method widely used in industry. The helium leakage rate test is carried out on a self-built device. Fig. 9 It is a schematic diagram of a helium leakage rate testing device, comprising a helium cylinder 1, a pressure sensor 2, a testing tool 3 and a suction gun 4, wherein the suction gun 4 is connected to a leak detector. Fig.10 yes Fig. 9 A partial enlarged view of the test fixture 3 of the helium leakage rate test device, including an elastic sealing ring 5, a helium inlet 6, a cavity 7, a test sample 8, a bolt-fastened cover plate 9 and a helium outlet 10. Fig. 9 , Fig.10 The helium leakage rate test is carried out as follows: the test medium is helium (He), the sample 8 is placed in the test fixture 3, the helium inlet 6 of the test fixture 3 is connected to the helium cylinder 1, and the helium inlet 6 is set to a certain pressure P 进口 , the helium outlet 10 can be opened to put the sample 8 under test, and then the outlet 10 can be covered by the bolt-tightening cover plate 9. The protruding sealing rod on the bolt-tightening cover plate 9 can be equipped with an elastic sealing ring 5, and the part of the sealing rod that contacts the sample 8 under test has a leakage hole leading to the atmosphere. Helium is introduced into the cavity 7 and the pressure is maintained for, for example, 3 minutes. The reading changes of the helium leak detector are monitored. If there is helium leakage in the sample 8 under test, it can be sniffed by the helium leak detector connected to the sniffer 4, and the real-time leakage rate under static pressure can be read through the digital display screen equipped on the helium leak detector.

[0075] The porous carbon block material of the present invention preferably has a high compressive strain (≥5%) and the compressive strain returns to zero after the stress is removed, that is, it exhibits many properties similar to rubber, and can therefore be called "rubber-like carbon". Preferably, the porous carbon block material has "high elasticity", and more preferably, the rubber-like carbon described herein also has a very low helium leakage rate as described herein, preferably "high sealing" or "high air tightness". Further preferably, the rubber-like carbon described herein also has a density as described herein, preferably "lightweight". Through transmission electron microscopy observation, the porous carbon block material of the present invention presents a three-dimensional porous structure with curved multilayer graphene as the pore boundary. Specifically, it is composed of multilayer graphene sheets that are chaotically arranged and cross-linked with each other and a large number of nanoscale pores formed between the graphene sheets, and these pores are closed. Herein, the "high sealing" or "high air tightness" of the porous carbon block material can be attributed to having such a rubber-like carbon structure. Preferably, there are basically no micrometer-sized pores in the porous carbon block material of the present invention.

[0076] In this article, the “high sealing property” of the porous carbon block material refers to the helium leakage rate of the porous carbon block material being no higher than 5×10 -5 Pa·m 3 / s.

[0077] In this article, the "high elasticity" of the porous carbon block material refers to the compressive strain of the porous carbon block material ≥ about 5%, preferably ≥ about 7%, and more preferably ≥ about 10%. Therefore, it is particularly preferred that the compressive strain of the porous carbon block material of the present application is ≥ 10%. More preferably, the compressive strain of the porous carbon block material returns to zero after the stress is removed.

[0078] In this context, the porous carbon block material is “lightweight”, which means that the density of the porous carbon block material is very low, for example, 0.3-1.1 g / cm 3 , preferably 0.4-1.0g / cm 3 , more preferably 0.5-0.9 g / cm 3 , especially preferably not higher than 0.7 g / cm 3 , for example, 0.5-0.7 g / cm 3 .

[0079] According to a second aspect of the present invention, there is provided a method for preparing the porous carbon block material according to the first aspect of the present invention, comprising:

[0080] A) Amorphous carbon-coated diamond nanoparticles as precursor powder;

[0081] B) placing the precursor powder of step A) into a mold and pre-pressing to obtain a pre-pressed green body;

[0082] C) placing the pre-pressed green body obtained in step B) into a sintering mold, and then placing the sintering mold containing the pre-pressed green body into a sintering device, applying sintering pressure, and then heating to a sintering temperature, maintaining the temperature, and sintering, wherein:

[0083] The sintering pressure is 5-100MPa,

[0084] The sintering temperature is 1000-2000℃,

[0085] The heating rate is 5-200℃ / min,

[0086] The insulation time is 0-30min;

[0087] D) Take out the mold, demould, and obtain a porous carbon block material.

[0088] In a preferred embodiment of the method of the present invention, the grain size of the amorphous carbon-coated diamond nanoparticles in step A) is 5-400 nm, preferably 5-350 nm, and more preferably 5-300 nm.

[0089] In step B) of the method of the present invention, the pre-pressing is performed by applying pressure in both directions. Preferably, the pressure applied in the pre-pressing is 1-20 MPa, preferably 2-15 MPa, more preferably 2-10 MPa, and most preferably 2-5 MPa. Preferably, the holding time of the pre-pressing is 1-20 min, preferably 1-15 min, more preferably 1-10 min, and most preferably 1-5 min.

[0090] In step C) of the method of the present invention, the pre-pressed green body obtained in step B) is placed in a sintering mold, and then the sintering mold containing the pre-pressed green body is placed in a sintering device, and sintering pressure is applied to perform sintering.

[0091] In a preferred embodiment of the method of the present invention, the sintering in step C) is spark plasma sintering or hot pressing sintering. In this article, spark plasma sintering or hot pressing sintering can be carried out using known equipment, for example, commercially available equipment can be used, such as SPS-3.20MK-I spark plasma sintering equipment purchased from Sumitomo Coal Mining Co., Ltd. or HIGH-MULTI-5000 hot pressing sintering equipment purchased from Fuji Electric Industries, Ltd. of Japan.

[0092] In a preferred embodiment of the method of the present invention, the sintering pressure in step C) can be set to 5-100 MPa, preferably 8-150 MPa, and more preferably 10-100 MPa. Within the pressure range, it is possible to obtain a high-strength sintered body at a relatively low temperature, apply less pressure, reduce industrial costs, and facilitate industrial mass production. At the same time, the pressure range can control the phase change speed of the diamond nanopowder and prevent the grains from growing too fast.

[0093] In a preferred embodiment of the method of the present invention, the sintering temperature in step C) can be set to 1000-2000°C, more preferably 1400-2000°C.

[0094] In a preferred embodiment of the method of the present invention, the heating rate in step C) can be set to 8-150° C. / min, more preferably 10-100° C. / min.

[0095] In a preferred embodiment of the method of the present invention, the holding time in step C) can be set to 0-20 min, more preferably 0-15 min.

[0096] In step C) of the method of the present invention, preferably, the sintering mold is a graphite mold, and the periphery of the graphite mold is wrapped with carbon felt. Preferably, the sintering mold is a graphite mold, and the pre-pressed body and the graphite mold are separated by graphite paper, and the periphery of the graphite mold is wrapped with carbon felt. The periphery of the graphite mold is wrapped with carbon felt, and the carbon felt surrounds the gap in the middle of the graphite mold, which can reduce the heat diffusion in the graphite mold and reduce the temperature gradient inside the graphite mold, thereby avoiding the uneven microstructure and mechanical properties of the sintered body.

[0097] Preferably, in step C) of the method of the present invention, an initial pressure of 2-10 MPa is optionally applied before the sintering step, and the vacuum is evacuated to a vacuum degree higher than 1×10 -1 Pa, and then apply sintering pressure.

[0098] In a preferred embodiment of the method of the present invention, in step C), after the sintering pressure is stabilized at a preset value, the temperature is raised to the sintering temperature, the temperature is maintained, and sintering is performed.

[0099] Preferably, after sintering is completed and before step D), step C') is included: cooling and decompressing to normal pressure, preferably, the cooling rate is 100-1000° C. / min.

[0100] In each embodiment, preferred embodiment, more preferred embodiment, etc. of the method of the present invention, the testing methods for various parameters such as pore size, porosity, density, compressive strain, compressive strength, helium leakage rate, etc. of the porous carbon block material are the same as the methods described for the porous carbon block material of the first aspect of the present invention, and will not be repeated here.

[0101] The porous carbon block material prepared by the method of the present invention is the rubber-like carbon described for the porous carbon block material of the first aspect of the present invention. The specific structure is as described above and will not be repeated here.

[0102] Example

[0103] The present invention is further described in detail below with reference to the embodiments.

[0104] Material

[0105] Amorphous carbon-coated nanodiamond powder with a grain size of 5-300 nm was purchased from Inokai Technology Co., Ltd.

[0106] Instruments and Equipment

[0107] X-ray diffractometer, Bruker D8 Advance.

[0108] Transmission electron microscope, Talos F200X model, was purchased from ThermoFisher Scientific Company.

[0109] Scanning electron microscope, Helios 5 model, was purchased from ThermoFisher Scientific.

[0110] Material mechanical properties testing machine, model TE-3000, was purchased from Jinan Jinyinfeng Instrument Co., Ltd.

[0111] The helium leak rate tester is a self-built device, and its detailed description is given above and in the “Performance Test” section below.

[0112] Spark plasma sintering equipment, SPS-3.20MK-I, was purchased from Sumitomo Coal Mining Co., Ltd.

[0113] The hot pressing sintering equipment, HIGH-MULTI-10000, was purchased from Fuji Electric Industries, Japan.

[0114] Example 1

[0115] The porous carbon block material was prepared according to the following steps:

[0116] A) Ingredients: Weigh 1 g of amorphous carbon-capped diamond nanoparticles as precursor powder.

[0117] B) Charging: The precursor powder weighed in step A) is placed in a mold with an inner diameter of 15 mm, and pre-pressed by applying pressure in both directions. The pressure is 5 MPa, and the holding time is 5 min. After pre-pressing, a pre-pressed blank is obtained;

[0118] C) Sintering: The pre-pressed green body obtained in step B) is placed in a graphite mold for sintering, the pre-pressed green body and the graphite mold are separated by graphite paper, and the periphery of the graphite mold is wrapped with carbon felt to obtain a sintering mold containing the pre-pressed green body; then, the sintering mold containing the pre-pressed green body is placed in a spark plasma sintering device, spark plasma sintering is performed, an initial pressure of 5 MPa is applied, and vacuum is evacuated to a vacuum degree of 5×10 -1Pa, then apply 10MPa sintering pressure, and after the sintering pressure stabilizes, heat up to sintering temperature 1400℃, heating rate is 100℃ / min, keep warm for 1min, sinter, turn off heating program after sintering, cool down and release pressure;

[0119] D) Discharging: After the temperature in the equipment cools down, the mold is taken out and demoulding is performed to obtain a porous carbon block material.

[0120] Example 2

[0121] A porous carbon block material is prepared by a method similar to that of Example 1, except that hot pressing sintering is used, wherein various parameters for hot pressing sintering are listed in Table 1.

[0122] Example 3

[0123] A porous carbon block material was prepared by a method similar to that of Example 1, except that the parameters of spark plasma sintering were changed. The specific parameters of this example are listed in Table 1.

[0124] Table 1 Method parameters of Examples 1-3

[0125]

[0126] Performance Testing

[0127] The following performance tests are all carried out at room temperature and normal pressure.

[0128] The compressive strength and compressive strain were tested on a mechanical properties testing machine according to the method described in GB / T 8489-2006. The test sample was a cylinder with a diameter of 3 mm and a height of 4.5 mm. The loading strain rate of the material mechanical properties testing machine was 5×10 -4 .

[0129] Density is obtained by dividing the sample mass by the volume. First, the sample is processed into a cylinder with a diameter of 20 mm and a height of 5 mm, and the volume V is calculated according to the cylinder volume calculation formula. 样品 , and then use a high-precision electronic balance to test the sample mass m 样品 . Sample density ρ 样品 =m 样品 / V 样品 .

[0130] The porosity is calculated based on the density of the sample obtained from the test and the theoretical density of graphite. Specifically, the porosity calculation method is as follows:

[0131] k=1-ρ 样品 / ρ 石墨 ,

[0132] Where k is the porosity, ρ 样品is the density of the sample, ρ 石墨 is the theoretical density of graphite (2.26 g / cm 3 ).

[0133] Transmission electron microscopy image: The sample was crushed using an agate mortar and ultrasonically dispersed in alcohol. The alcohol-sample mixture was then allowed to stand for 10 minutes. A dropper was used to take the upper clear liquid and drop it on the copper microgrid. After the alcohol on the microgrid evaporated, the microgrid with the sample powder was placed in a transmission electron microscope for observation.

[0134] The pore sizes are measured directly from high-resolution transmission electron microscopy images in randomly selected representative areas of the material.

[0135] The sealing of the sample is characterized by testing its helium leakage rate. Helium is one of the smallest gas molecules and can quickly penetrate small leaks. It is chemically inert, does not react with any material in the tested part, and only exists in trace amounts (5ppm) in the atmosphere. Using helium leakage rate to characterize the airtightness of devices and components has become a high-precision airtightness test method widely used in industry. Helium leakage rate test is carried out on a self-built device (see Fig. 9 , Fig.10 ) is carried out as follows: the test medium is helium (He), the sample 8 to be tested is placed in the test fixture 3, the helium inlet 6 of the test fixture 3 is connected to the helium cylinder 1, and the helium inlet 6 is set to a certain pressure P 进口 , the helium outlet 10 can be opened to put the sample 8 under test, and then the outlet 10 can be covered with a bolted cover plate 9. The protruding sealing rod on the bolted cover plate 9 can be equipped with an elastic sealing ring 5, and the part of the sealing rod that contacts the sample 8 under test has a leakage hole leading to the atmosphere. Helium is introduced into the cavity 7 and the pressure is maintained for 3 minutes. Monitor the reading changes of the helium leak detector. If there is helium leakage in the sample 8 under test, it can be sniffed by the helium leak detector connected to the sniffer 4, and the real-time leakage rate under static pressure can be read through the digital display screen equipped on the helium leak detector.

[0136] Test Results

[0137] Aperture size

[0138] The pore sizes of the porous carbon block materials prepared in Examples 1-3 were measured according to the above method, and the test results are listed in Table 2. It can be seen that the porous carbon block material of the present invention has a small pore size.

[0139] Porosity

[0140] The porosity of the porous carbon block material prepared in Examples 1-3 was measured and calculated according to the above method, and the test results are listed in Table 2. It can be seen that the porous carbon block material of the present invention has a high porosity.

[0141] density

[0142] like Figure 1 As shown in (a), the porous carbon block material prepared in Example 1 is an opaque black block. Figure 1 As shown in (b), the porous carbon block material prepared in Example 1 floats in water, and it can be clearly observed that the density of the sample is less than the density of water (1 g / cm 3 ), measured according to the above method, the density of the porous carbon block material prepared in Example 1 is 0.5 g / cm 3 The porous carbon block materials prepared in Example 2 and Example 3 have similar shapes and densities that are also less than water, see Table 2.

[0143] Helium leakage rate

[0144] The helium leakage rates of the porous carbon block materials prepared in Examples 1-3 were tested by the above method and are listed in Table 2. It can be seen that the helium leakage rate of the porous carbon block material of the present invention is extremely low, and thus has very high air tightness.

[0145] According to the helium leakage rate test, it can be seen that the helium leakage rate of the porous carbon block material in each embodiment is ≤2×10 -5 Pa·m 3 / s, which is equivalent to the helium leakage rate of rubber (1×10 -5 Pa·m 3 / s). The helium leakage rate test results directly show that the material of the present application has high airtightness characteristics and can be used as a sealing material. In addition, it also proves that the pores in the porous carbon material of the present application are closed pores.

[0146] Morphology and structure

[0147] The porous carbon block materials prepared in Examples 1-3 were analyzed using an X-ray diffractometer. Figure 2 As shown, it can be seen that the amorphous carbon-wrapped nanodiamonds in the porous carbon block materials prepared in Examples 1-3 have completely transformed into a turbostratic graphite structure.

[0148] Figure 3 and Figure 4This is a transmission electron microscopic image of the porous carbon block material prepared in Example 1. It can be seen that the prepared carbon block material is composed of chaotically arranged multilayer graphene. The curved graphene is entangled and cross-linked with each other to form a large number of closed pores with a pore size between 5-30nm. Since these holes are closed pores, the prepared porous carbon block material has a very low helium leakage rate. The porous carbon block materials prepared in Example 2 and Example 3 have similar organizational structures and therefore also have a very low helium leakage rate. The helium leakage rates of the porous carbon block materials prepared in Examples 1-3 are listed in Table 2.

[0149] Figure 5 is a scanning electron microscope image of the porous carbon block material prepared in Example 1. Figure 5 As shown, the cross-sectional surface of the porous carbon block material prepared by the present invention is flat, which indicates that the pores inside the porous carbon block material are relatively small and no pores can be observed under a scanning electron microscope. The porous carbon block materials prepared in Examples 2 and 3 have pores of similar size.

[0150] Compressive Strength and Compressive Strain

[0151] Figure 6 (a) shows the single compression stress-strain curve of the porous carbon block material prepared in Example 1, with a compressive strength of 175 MPa and a compressive strain of 12.2%. The stress-strain curve has obvious nonlinear characteristics. Figure 7 (a) shows the cyclic compression stress-strain curve of the product prepared in Example 1, with the highest compressive strength being 168 MPa, the maximum compressive strain being 11%, and the strain of the sample being completely recovered after the stress is removed, indicating that the sample is a purely elastic deformation. Figure 5 This is the cyclic compression stress-strain curve of the porous carbon block material prepared in Example 1 measured at 600°C in an air atmosphere. The elastic behavior is basically maintained at high temperature.

[0152] Figure 6 (b) shows a single compression stress-strain curve of the porous carbon block material prepared in Example 2, with a compressive strength of 240 MPa and a compressive strain of 9.8%. The stress-strain curve has obvious nonlinear characteristics. Figure 7 (b) shows the cyclic compressive stress-strain curve of the porous carbon block material prepared in Example 2, with the highest compressive strength being 225 MPa, the maximum compressive strain being 8%, and the strain of the sample returning to zero after the stress is removed.

[0153] like Figure 6 (c) shows the single compression stress-strain curve of the porous carbon block material prepared in Example 3, with a compression strength of 301 MPa and a compression strain of 7.7%. The stress-strain curve has obvious nonlinear characteristics. Figure 7(c) shows the cyclic compressive stress-strain curve of the porous carbon block material prepared in Example 3, with the highest compressive strength being 285 MPa, the maximum compressive strain being 7%, and the strain of the sample returning to zero after the stress is removed.

[0154] Table 2 Properties of porous carbon block materials prepared in Examples 1-3

[0155]

[0156] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

[0157] The optional materials of various components are listed in the description of the present invention, but those skilled in the art should understand that the above-mentioned list of component materials is not limiting and not exhaustive, and various components can be replaced by other equivalent materials not mentioned in the description of the present invention, while still achieving the purpose of the present invention. The specific examples mentioned in the description are also for the purpose of explanation only, not for limiting the scope of the present invention.

[0158] In addition, the dosage range of each component of the present invention includes any combination of any lower limit and any upper limit mentioned in the specification, and also includes any range formed by the specific content of the component in each specific embodiment as an upper limit or a lower limit combination; all these ranges are included in the scope of the present invention, but these combined ranges are not listed one by one in the specification just to save space. Each feature of the present invention listed in the specification can be combined with any other feature of the present invention, and such combination is also within the scope of the disclosure of the present invention; these combined ranges are not listed one by one in the specification just to save space.

Claims

1. A porous carbon block material, wherein: The pore size of the porous carbon block material is in the range of 3-100 nm; The porosity of the porous carbon block material is 56-87%; The density of the porous carbon block material is 0.3-1.1 g / cm 3 ; The pores in the porous carbon block material are closed pores; The compressive strain of the porous carbon block material is ≥5%; and / or the compressive strength of the porous carbon block material is >100 MPa; and Observation through a transmission electron microscope shows that the porous carbon block material presents a three-dimensional porous structure with curved multilayer graphene as pore boundaries.

2. The porous carbon block material according to claim 1, wherein: The pore size of the porous carbon block material is in the range of 5-50 nm.

3. The porous carbon block material according to claim 1, wherein: The pore size of the porous carbon block material is in the range of 5-30 nm.

4. The porous carbon block material according to claim 1, wherein: The porosity of the porous carbon block material is 56-82%.

5. The porous carbon block material according to claim 1, wherein: The porosity of the porous carbon block material is 60-80%.

6. The porous carbon block material according to claim 1, wherein: The compressive strain of the porous carbon block material is ≥6%.

7. The porous carbon block material according to claim 1, wherein: The compressive strain of the porous carbon block material is ≥7%.

8. The porous carbon block material according to claim 1, wherein: The compressive strength of the porous carbon block material is greater than 150 MPa.

9. The porous carbon block material according to any one of claims 1 to 5, wherein: The helium leakage rate of the porous carbon block material is ≤10×10 -5 Pa·m 3 / s.

10. The porous carbon block material according to claim 9, wherein: The helium leakage rate of the porous carbon block material is ≤4×10 -5 Pa·m 3 / s.

11. The porous carbon block material according to claim 9, wherein: The helium leakage rate of the porous carbon block material is ≤2×10 -5 Pa·m 3 / s.

12. The porous carbon block material according to claim 1, wherein: The density of the porous carbon block material is 0.4-1.0 g / cm 3 .

13. The porous carbon block material according to claim 1, wherein: The density of the porous carbon block material is 0.5-0.9 g / cm 3 .

14. The method for preparing the porous carbon block material according to claim 1, comprising: A) Amorphous carbon-coated diamond nanoparticles as precursor powder; B) placing the precursor powder of step A) into a mold and pre-pressing to obtain a pre-pressed green body; C) placing the pre-pressed green body obtained in step B) into a sintering mold, and then placing the sintering mold containing the pre-pressed green body into a sintering device, applying sintering pressure, and then heating to a sintering temperature, maintaining the temperature, and sintering, wherein: The sintering pressure is 5-100MPa, The sintering temperature is 1300-2000℃; D) Take out the mold, demould, and obtain a porous carbon block material.

15. The method for preparing the porous carbon block material according to claim 14, wherein: The grain size of the amorphous carbon-coated diamond nanoparticles is 5-400 nm.

16. The method for preparing the porous carbon block material according to claim 14, wherein: The grain size of the amorphous carbon-coated diamond nanoparticles is 5-350 nm.

17. The method for preparing the porous carbon block material according to claim 14, wherein: The grain size of the amorphous carbon-coated diamond nanoparticles is 5-300 nm.

18. The method for preparing the porous carbon block material according to claim 14, wherein: The sintering is spark plasma sintering or hot pressing sintering.

19. The method for preparing the porous carbon block material according to claim 14 or 18, wherein: The sintering pressure is 5-80 MPa.

20. The method for preparing the porous carbon block material according to claim 19, wherein: The sintering pressure is 10-70MPa.

21. The method for preparing the porous carbon block material according to claim 14, wherein: The sintering temperature is 1400-2000℃.

22. The method according to claim 14, wherein: In step B), the pre-pressing is performed by applying pressure in both directions, the applied pressure is 1-20 MPa, and the holding time is 1-20 min.

23. The method according to claim 22, wherein: The applied pressure is 2-15 MPa.

24. The method according to claim 22, wherein: The applied pressure is 2-10 MPa.

25. The method according to claim 22, wherein: The applied pressure is 2-5 MPa.

26. The method of claim 22, wherein: The holding time is 1-15min.

27. The method of claim 22, wherein: The holding time is 1-10min.

28. The method of claim 22, wherein: The holding time is 1-5min.

29. The method of claim 14, wherein: The sintering mold in step C) is a graphite mold, wherein the pre-pressed green body and the graphite mold are separated by graphite paper, and the periphery of the graphite mold is wrapped with carbon felt.

30. The method of claim 14, wherein: In step C), before applying the sintering pressure, an initial pressure of 2-10 MPa is optionally applied, and the vacuum is evacuated to a vacuum degree higher than 1×10 -1 Pa, and then apply sintering pressure.

31. The method of claim 14, wherein: In step C), after the sintering pressure is stabilized at a preset value, the temperature is raised to the sintering temperature, the temperature is maintained, and sintering is performed.

32. The method of claim 14, wherein: After the sintering is completed, before step D), the process comprises step C): cooling and decompressing to normal pressure.

33. The method of claim 32, wherein: The cooling rate is 100-1000°C / min.

34. The method of claim 14, wherein: In step C), the heating rate is 5-200° C. / min; and the holding time is 0-30 min.

35. The method of claim 34, wherein: The heating rate is 8-150℃ / min.

36. The method of claim 34, wherein: The heating rate is 10-100°C / min.

37. The method of claim 34, wherein: The insulation time is 0-20min.