Isolated island structure TiB2 / Cu-Cu composite material and preparation method thereof

Through the preparation method of the isolated island-like structure TiB2/Cu-Cu composite, the problem of poor plastic/toughness caused by the non-uniform distribution of TiB2 particles in Cu-based composite materials is solved, and the mechanical properties and electrical conductivity of the material are significantly improved.

CN115927895BActive Publication Date: 2024-11-22XIAN UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211399651.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-09
Publication Date
2024-11-22
Estimated Expiration
2042-11-09

AI Technical Summary

Technical Problem

The non-uniform distribution of TiB2 particles in Cu-based composite materials leads to poor plastic/toughness of the material, limiting the improvement of its comprehensive performance.

Method used

The preparation method of the isolated island-like structure TiB2/Cu-Cu composite material is adopted, and the spherical Cu+TiH2+B precursor powder is generated by ball mill mechanical alloying treatment and vibration powder mixing technology, followed by cold press forming and hot pressing sintering to form TiB2 The /Cu composite zone is isolated island-like structure wrapped by a pure Cu zone.

Benefits of technology

It significantly improves the mechanical properties and conductivity of TiB2/Cu composite materials, solves the problem of poor plastic/toughness, and improves the cold working deformation ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115927895B_ABST
    Figure CN115927895B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an isolated island structure TiB2 / Cu-Cu composite material, which specifically includes the following steps: Step 1: first, Cu powder, TiH2 powder, and B powder are weighed in proportion according to the pre-generated amount of TiB2 particles in the composite material, and then mechanically alloyed by a ball mill to obtain a spherical Cu+TiH2+B precursor powder; Step 2: Spherical Cu+TiH2+B precursor powder and pure Cu powder are mixed in proportion by a vibrating powder mixing device; Step 3: The mixed powder fully mixed in step 2 is cold pressed to obtain a cold pressed blank; Step 4: The pressed blank is placed in a graphite mold for hot pressing and sintering to prepare an isolated island structure TiB2 / Cu-Cu composite material. The method solves the problem of poor plasticity / toughness of TiB2 particle dispersion-enhanced Cu-based composite materials. An isolated island structure TiB2 / Cu-Cu composite material is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal matrix composite materials, and in particular relates to an isolated island structure TiB2 / Cu-Cu composite material, and also relates to a preparation method of the isolated island structure TiB2 / Cu-Cu composite material. Background Art

[0002] Discontinuous particle reinforced metal matrix composites have become indispensable lightweight structural materials and functional materials in high-tech fields such as military defense, aerospace, and rail transportation due to their advantages in cost, mechanical properties, specific strength, thermal stability, isotropy, and machining. However, although these metal matrix composites have many favorable properties such as high conductivity, high thermal stability, and high strength, the addition of a large number of discontinuous brittle ceramic particles in the matrix still greatly reduces the room temperature damage tolerance (toughness, ductility, and defect sensitivity) of the material, so that it cannot be more widely used. At present, the focus of attention in this field is to control the volume fraction, size, and aspect ratio of the reinforcement in the metal matrix to obtain a metal matrix composite with uniformly dispersed reinforcement. However, theoretical analysis and research results have shown that the configuration design of non-uniform distribution of reinforcement in the matrix is ​​expected to break the bottleneck of poor damage tolerance of the material. In recent years, TiB2 particle reinforced Cu-based composites have been used as the preferred material for high-strength and high-conductivity metal structural components. The limited improvement of its comprehensive performance caused by the dispersed distribution of reinforcement has also become a key problem to be solved in this field. Summary of the invention

[0003] The first object of the present invention is to provide a method for preparing an isolated island structure TiB2 / Cu-Cu composite material, which solves the problem of poor plasticity / toughness of TiB2 particle dispersion reinforced Cu-based composite materials and further improves the comprehensive performance of TiB2 / Cu composite materials.

[0004] The second object of the present invention is to provide an isolated island structure TiB2 / Cu-Cu composite material, which solves the problem of poor plasticity / toughness of TiB2 particle dispersion reinforced Cu-based composite materials.

[0005] The first technical solution adopted by the present invention is a method for preparing an isolated island structure TiB2 / Cu-Cu composite material, which specifically comprises the following steps:

[0006] Step 1: First, Cu powder, TiH2 powder and B powder are weighed according to the pre-generated amount of TiB2 particles in the composite material, and then mechanically alloyed by a ball mill to obtain a spherical Cu+TiH2+B precursor powder;

[0007] Step 2: Mix the spherical Cu+TiH2+B precursor powder and pure Cu powder in proportion by using a vibration powder mixing device;

[0008] Step 3: cold pressing the mixed powder mixed thoroughly in step 2 to obtain a cold pressed blank;

[0009] Step 4: placing the compact in a graphite mold for hot pressing and sintering to prepare an isolated island structure TiB2 / Cu-Cu composite material.

[0010] The present invention is also characterized in that

[0011] The specific implementation method of step 1 is:

[0012] Firstly, the proportion of TiH2 powder and B powder was calculated based on the molar ratio of Ti atoms to B atoms of 1:2, and the content of in-situ generated TiB2 particles accounted for 1wt.%-5wt.% of the Cu+TiH2+B precursor powder. Cu powder, TiH2 powder and B powder were weighed respectively, and then the three raw material powders were inverted into the same ball mill at the same time, and the ball mill beads were weighed according to the mass of the powder in the ball mill at a ball-to-material ratio of 10:1-20:1. Anhydrous ethanol was added as a process control agent according to 1wt.%-3wt.% of the mass of the powder in the ball mill, and then the ball mill was evacuated to 1.0×10 -2 Pa and then filled with argon to a low negative pressure, which was repeated several times to ensure that the ball mill was completely protected by the argon atmosphere; finally, the ball mill was placed in a ball mill for ball milling at a speed of 350r / min-450r / min and a ball milling time of 5h-20h to obtain spherical Cu+TiH2+B precursor powder.

[0013] In step 1, the particle size of the spherical Cu+TiH2+B precursor powder ranges from 200 to 900 μm.

[0014] In step 2, the spherical Cu+TiH2+B precursor powder and the pure Cu powder are vibrated and mixed at a mass ratio of 4:1-1:4 to obtain a mixed powder of spherical Cu+TiH2+B precursor powder and pure Cu powder, wherein the frequency of the vibration mixing is 30Hz-50Hz, and the vibration time is 1h-3h.

[0015] The specific implementation of step 3 is:

[0016] The mixed powder obtained in step 2 is weighed and placed in a quenched steel cold pressing mold, and is cold pressed by a four-column hydraulic press with a loading pressure of 50MPa-200MPa and a holding time of 20s-60s to obtain a cold pressed billet with a higher density.

[0017] The specific implementation of step 4 is:

[0018] The cold pressed blank is loaded into a graphite crucible and placed in the center of a sintering furnace. The cover of the hot pressing furnace is closed for sintering. The sintering atmosphere is inert gas protection or vacuum. The sintering process is first heated to 850-950°C at a rate of 10-30°C / min and kept warm for 0.5-1h. The temperature is then continued to be raised to 950-1060°C and kept warm for 0.5-2h at a pressure of 0-50MPa. The blank is then cooled to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

[0019] The second technical solution adopted by the present invention is that the isolated island structure TiB2 / Cu-Cu composite material is prepared by the above method.

[0020] The beneficial effects of the present invention are:

[0021] The present invention discloses a method for preparing an isolated island structure TiB2 / Cu-Cu composite material, wherein the macroscopic structure of the composite material is an isolated island structure in which a TiB2 / Cu composite area is wrapped by a pure Cu area, and the pure Cu area is spatially connected. The isolated island structure TiB2 / Cu composite material not only exhibits excellent cold working deformation ability, but also solves the problem of poor plasticity / toughness of the TiB2 particle dispersion reinforced Cu-based composite material, and significantly improves the mechanical properties and electrical conductivity of the TiB2 / Cu composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The morphology of the spherical Cu+TiH2+B precursor powder after ball milling in Example 1 of the present invention;

[0023] Figure 2 The sintered morphology of the isolated island structure TiB2 / Cu-Cu composite material prepared in Example 1 of the present invention;

[0024] Figure 3 The sintered morphology of the isolated island structure TiB2 / Cu-Cu composite material obtained in Example 2 of the present invention;

[0025] Figure 4 The composite zone microstructure of the sintered TiB2 / Cu-Cu composite material with isolated island structure obtained in Example 2 of the present invention;

[0026] Figure 5 The rolled morphology of the isolated island structure TiB2 / Cu-Cu composite material obtained in Example 3 of the present invention. DETAILED DESCRIPTION

[0027] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0028] The present invention provides a method for preparing an isolated island structure TiB2 / Cu-Cu composite material, which specifically comprises the following steps:

[0029] Step 1: First, Cu powder, TiH2 powder and B powder are weighed according to the pre-generated amount of TiB2 particles in the composite material, and then mechanically alloyed by a ball mill to obtain a spherical Cu+TiH2+B precursor powder;

[0030] The specific implementation method of step 1 is:

[0031] Firstly, the proportion of TiH2 powder and B powder was calculated based on the molar ratio of Ti atoms to B atoms of 1:2, and the content of in-situ generated TiB2 particles accounted for 1wt.%-5wt.% of the Cu+TiH2+B precursor powder. Cu powder, TiH2 powder and B powder were weighed respectively, and then the three raw material powders were inverted into the same ball mill at the same time, and the ball mill beads were weighed according to the mass of the powder in the ball mill at a ball-to-material ratio of 10:1-20:1. Anhydrous ethanol was added as a process control agent according to 1wt.%-3wt.% of the mass of the powder in the ball mill, and then the ball mill was evacuated to 1.0×10 -2 Pa, and then filled with argon to a low negative pressure, and repeated several times to ensure that the ball mill is completely protected by the argon atmosphere; finally, the ball mill is placed in a ball mill for ball milling at a speed of 350r / min-450r / min and a ball milling time of 5h-20h to obtain a spherical Cu+TiH2+B precursor powder. In step 1, the particle size range of the spherical Cu+TiH2+B precursor powder is 200-900μm.

[0032] Step 2: Mix the spherical Cu+TiH2+B precursor powder and pure Cu powder in proportion by using a vibration powder mixing device;

[0033] In step 2, the spherical Cu+TiH2+B precursor powder and the pure Cu powder are subjected to three-dimensional vibration mixing at a mass ratio of 4:1-1:4 to obtain a mixed powder of the spherical Cu+TiH2+B precursor powder and the pure Cu powder, wherein the frequency of the vibration mixing is 30Hz-50Hz and the vibration time is 1h-3h. Step 3: The mixed powder mixed thoroughly in step 2 is cold pressed to obtain a cold pressed blank;

[0034] The specific implementation of step 3 is:

[0035] The mixed powder obtained in step 2 is weighed and placed in a quenched steel cold pressing mold, and is cold pressed by a four-column hydraulic press with a loading pressure of 50MPa-200MPa and a holding time of 20s-60s to obtain a cold pressed billet with a higher density.

[0036] Step 4: placing the compact in a graphite mold for hot pressing and sintering to prepare an isolated island structure TiB2 / Cu-Cu composite material.

[0037] The specific implementation of step 4 is:

[0038] The cold pressed blank is loaded into a graphite crucible and placed in the center of a sintering furnace. The cover of the hot pressing furnace is closed for sintering. The sintering atmosphere is inert gas protection or vacuum. The sintering process is first heated to 850-950°C at a rate of 10-30°C / min and kept warm for 0.5-1h. The temperature is then continued to be raised to 950-1060°C and kept warm for 0.5-2h at a pressure of 0-50MPa. The blank is then cooled to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

[0039] Example 1

[0040] Step 1: Cu powder, TiH2 powder and B powder are mixed according to the content of TiB2 particles generated by in-situ reaction accounting for 2wt.% of the precursor powder matrix, and then the masses of Cu powder, TiH2 powder and B powder are weighed to be 29.4g, 0.43g and 0.19g respectively, and then the three raw material powders are inverted in the same ball mill at the same time, and then added into the same ball mill together with ball milling beads and anhydrous ethanol and evacuated to 1.0×10 -2 Pa and then filled with argon to a low negative pressure, which was repeated several times to ensure that the ball mill was completely protected by the argon atmosphere, and then the ball mill was placed in a ball mill for ball milling at 450 r / min for 8 hours, wherein the mass of the grinding balls was 15 times the mass of the powder in the ball mill, and the amount of anhydrous ethanol added as a process control agent was 3 wt.%, and finally spherical Cu+TiH2+B precursor powder was obtained.

[0041] Step 2: Weigh the spherical precursor powder and pure Cu powder in a weight ratio of 2:3, place them in a powder mixing tank and vibrate them for 1 hour at a frequency of 40 Hz to obtain a uniform mixed powder of the spherical precursor powder and pure Cu powder.

[0042] Step 3: Weigh the mixed powder obtained in step 2 and place it in a quenched steel cold pressing mold, and perform cold pressing molding on it with a loading pressure of 100 MPa and a holding pressure of 40 seconds using a four-column hydraulic press to obtain a cold pressed billet with a higher density.

[0043] Step 4: Place the cold pressed blank into a graphite crucible and place it in the center of the sintering furnace, close the hot pressing furnace cover, and sinter under nitrogen protection. The sintering process first heats up to 900°C at a rate of 20°C / min and keeps warm for 0.5h, then continues to heat up to 1000°C and keeps warm for 1h at a pressure of 35MPa, and finally cools to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

[0044] After the above process, the isolated island structure TiB2 / Cu-Cu composite material prepared in this embodiment has a sintered conductivity of 93% IACS, a tensile elongation at break of 34%, and a deformation amount of up to 90% during room temperature rolling.

[0045] like Figure 1 The figure shows the morphology of the spherical Cu+TiH2+B precursor powder after ball milling in Example 1. It can be seen that the precursor powder is spherical and has a high sphericity.

[0046] like Figure 2 As shown, it is the sintered morphology of the isolated island structure TiB2 / Cu-Cu composite material prepared in Example 1. It can be seen that the TiB2 / Cu composite area is distributed in the matrix in the shape of isolated islands, the distance between two adjacent TiB2 / Cu composite areas is large, and the pure Cu area is spatially connected. This isolated island structure TiB2 / Cu composite material not only exhibits excellent cold working deformation ability, but also solves the problem of poor plasticity / toughness of TiB2 particle dispersion reinforced Cu-based composite materials, and significantly improves the mechanical properties and conductivity of the TiB2 / Cu composite material.

[0047] Example 2

[0048] Step 1: Cu powder, TiH2 powder and B powder are mixed according to the content of TiB2 particles generated by in-situ reaction accounting for 2wt.% of the precursor powder matrix, and then the masses of Cu powder, TiH2 powder and B powder are weighed to be 29.4g, 0.43g and 0.19g respectively, and then the three raw material powders are inverted in the same ball mill at the same time, and then added into the same ball mill together with ball milling beads and anhydrous ethanol and evacuated to 1.0×10 -2 Pa and then filled with argon to a low negative pressure, which was repeated several times to ensure that the ball mill was completely protected by the argon atmosphere, and then the ball mill was placed in a ball mill for ball milling at 450 r / min for 10 hours, wherein the mass of the grinding balls was 20 times the mass of the powder in the ball mill, and the amount of anhydrous ethanol added as a process control agent was 2 wt.%, and finally spherical Cu+TiH2+B precursor powder was obtained.

[0049] Step 2: Weigh the spherical precursor powder and pure Cu powder in a weight ratio of 3:2, place them in a powder mixing tank and vibrate them for 1 hour at a frequency of 40 Hz to obtain a uniform mixed powder of the spherical precursor powder and pure Cu powder.

[0050] Step 3: Weigh the mixed powder obtained in step 2 and place it in a quenched steel cold pressing mold, and perform cold pressing molding on it with a loading pressure of 100 MPa and a holding pressure of 40 seconds using a four-column hydraulic press to obtain a cold pressed billet with a higher density.

[0051] Step 4: Place the cold pressed blank into a graphite crucible and place it in the center of the sintering furnace, close the hot pressing furnace cover, and sinter under nitrogen protection. The sintering process first heats up to 900°C at a rate of 20°C / min and keeps warm for 0.5h, then continues to heat up to 1050°C and keeps warm for 1h at a pressure of 35MPa, and finally cools to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

[0052] After the above process, the isolated island structure TiB2 / Cu-Cu composite material prepared in this embodiment has a sintered conductivity of 88% IACS, a tensile elongation at break of 31%, and a deformation amount of up to 70% during room temperature rolling.

[0053] like Figure 3 As shown, it is the sintered morphology of the isolated island structure TiB2 / Cu-Cu composite material prepared in Example 2. It can be seen that the TiB2 / Cu composite area is distributed in the matrix in the shape of isolated islands, the distance between two adjacent TiB2 / Cu composite areas is small, and the pure Cu area is spatially connected. This isolated island structure TiB2 / Cu composite material not only exhibits excellent cold working deformation ability, but also solves the problem of poor plasticity / toughness of TiB2 particle dispersion reinforced Cu-based composite materials, and significantly improves the mechanical properties and conductivity of the TiB2 / Cu composite material.

[0054] like Figure 4 As shown, the composite area morphology in the sintered matrix of the isolated island structure TiB2 / Cu-Cu composite material prepared in Example 2, it can be seen that fine TiB2 particles are dispersed in the composite area.

[0055] Example 3

[0056] Step 1: Cu powder, TiH2 powder and B powder are mixed according to the content of TiB2 particles generated by in-situ reaction accounting for 2wt.% of the precursor powder matrix, and then the masses of Cu powder, TiH2 powder and B powder are weighed to be 29.4g, 0.43g and 0.19g respectively, and then the three raw material powders are inverted in the same ball mill at the same time, and then added into the same ball mill together with ball milling beads and anhydrous ethanol and evacuated to 1.0×10-2 Pa and then filled with argon to a low negative pressure, which was repeated several times to ensure that the ball mill was completely protected by the argon atmosphere, and then the ball mill was placed in a ball mill for ball milling at 400 r / min for 10 hours, wherein the mass of the grinding balls was 20 times the mass of the powder in the ball mill, and the amount of anhydrous ethanol added as a process control agent was 3 wt.%, and finally spherical Cu+TiH2+B precursor powder was obtained.

[0057] Step 2: Weigh the spherical precursor powder and pure Cu powder in a weight ratio of 1:1, place them in a powder mixing tank and vibrate them for 1 hour at a frequency of 40 Hz to obtain a uniform mixed powder of the spherical precursor powder and pure Cu powder.

[0058] Step 3: Weigh the mixed powder obtained in step 2 and place it in a quenched steel cold pressing mold, and perform cold pressing molding on it with a loading pressure of 100 MPa and a holding pressure of 40 seconds using a four-column hydraulic press to obtain a cold pressed billet with a higher density.

[0059] Step 4: Place the cold pressed blank into a graphite crucible and place it in the center of the sintering furnace, close the hot pressing furnace cover, and sinter under nitrogen protection. The sintering process first heats up to 900°C at a rate of 20°C / min and keeps warm for 0.5h, then continues to heat up to 1020°C and keeps warm for 1h at a pressure of 35MPa, and finally cools to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

[0060] After the above process, the isolated island structure TiB2 / Cu-Cu composite material prepared in this embodiment has a sintered conductivity of 90% IACS, a tensile elongation at break of 32%, and a deformation amount of up to 80% during room temperature rolling.

[0061] like Figure 5 As shown, it is the rolled morphology of the isolated island structure TiB2 / Cu-Cu composite material prepared in Example 3. It can be seen that the TiB2 / Cu composite area is still distributed in the matrix in an isolated strip-shaped island shape, and the pure Cu area is spatially connected. This isolated island structure TiB2 / Cu composite material not only exhibits excellent cold working deformation ability, but also solves the problem of poor plasticity / toughness of TiB2 particle dispersion reinforced Cu-based composite materials, and significantly improves the mechanical properties and conductivity of the TiB2 / Cu composite material.

[0062] Example 4

[0063] Step 1: Cu powder, TiH2 powder and B powder are mixed according to the content of TiB2 particles generated by in-situ reaction accounting for 3wt.% of the precursor powder matrix, and then the masses of Cu powder, TiH2 powder and B powder are weighed to be 29.1g, 0.64g and 0.28g respectively, and then the three raw material powders are inverted in the same ball mill at the same time, and then added into the same ball mill together with ball milling beads and anhydrous ethanol and evacuated to 1.0×10 -2 Pa and then filled with argon to a low negative pressure, which was repeated several times to ensure that the ball mill was completely protected by the argon atmosphere, and then the ball mill was placed in a ball mill for ball milling at 450r / min for 10 hours, wherein the mass of the grinding balls was 15 times the mass of the powder in the ball mill, and the amount of anhydrous ethanol added as the process control agent was 3wt.%, and finally spherical Cu+TiH2+B precursor powder was obtained.

[0064] Step 2: Weigh the spherical precursor powder and pure Cu powder in a weight ratio of 2:3, place them in a powder mixing tank and vibrate them for 1 hour at a frequency of 40 Hz to obtain a uniform mixed powder of the spherical precursor powder and pure Cu powder.

[0065] Step 3: Weigh the mixed powder obtained in step 2 and place it in a quenched steel cold pressing mold, and perform cold pressing molding on it with a loading pressure of 100 MPa and holding pressure for 60 seconds using a four-column hydraulic press to obtain a cold pressed billet with higher density.

[0066] Step 4: Place the cold pressed blank into a graphite crucible and place it in the center of the sintering furnace, close the hot pressing furnace cover, and sinter under nitrogen protection. The sintering process first heats up to 900°C at a rate of 20°C / min and keeps warm for 0.5h, then continues to heat up to 1040°C and keeps warm for 1h at a pressure of 35MPa, and finally cools to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

[0067] After the above process, the isolated island structure TiB2 / Cu-Cu composite material prepared in this embodiment has a sintered conductivity of 91% IACS, a tensile elongation at break of 32.4%, and a deformation amount of up to 80% during room temperature rolling.

[0068] Example 5

[0069] Step 1: Cu powder, TiH2 powder and B powder are mixed according to the content of TiB2 particles generated by in-situ reaction accounting for 3wt.% of the precursor powder matrix, and then the masses of Cu powder, TiH2 powder and B powder are weighed to be 29.1g, 0.64g and 0.28g respectively, and then the three raw material powders are inverted in the same ball mill at the same time, and then added into the same ball mill together with ball milling beads and anhydrous ethanol and evacuated to 1.0×10-2 Pa and then filled with argon to a low negative pressure, which was repeated several times to ensure that the ball mill was completely protected by the argon atmosphere, and then the ball mill was placed in a ball mill for ball milling at 400 r / min and for 8 hours, wherein the mass of the grinding balls was 15 times the mass of the powder in the ball mill, and the amount of anhydrous ethanol added as the process control agent was 3 wt.%, and finally spherical Cu+TiH2+B precursor powder was obtained.

[0070] Step 2: Weigh the spherical precursor powder and pure Cu powder in a weight ratio of 3:2, place them in a powder mixing tank and vibrate them for 2 hours at a frequency of 50 Hz to obtain a uniform mixed powder of the spherical precursor powder and pure Cu powder.

[0071] Step 3: Weigh the mixed powder obtained in step 2 and place it in a quenched steel cold pressing mold, and perform cold pressing molding on it with a loading pressure of 150 MPa and a holding pressure of 60 seconds using a four-column hydraulic press to obtain a cold pressed billet with a higher density.

[0072] Step 4: Place the cold pressed blank into a graphite crucible and place it in the center of the sintering furnace, close the hot pressing furnace cover, and sinter under nitrogen protection. The sintering process first heats up to 900°C at a rate of 25°C / min and keeps warm for 1 hour, then continues to heat up to 1040°C and keeps warm for 1 hour at a pressure of 35MPa, and finally cools to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

[0073] Through the above process, the isolated island structure TiB2 / Cu-Cu composite material prepared in this embodiment has a sintered conductivity of 87% IACS, a tensile elongation at break of 29%, and a deformation amount of up to 70% during room temperature rolling.

Claims

1. A method for preparing an isolated island structure TiB2 / Cu-Cu composite material, characterized in that: The specific steps include: Step 1: First, Cu powder, TiH2 powder and B powder are weighed according to the pre-generated amount of TiB2 particles in the composite material, and then mechanically alloyed by a ball mill to obtain a spherical Cu+TiH2+B precursor powder; The specific implementation method of step 1 is: Firstly, the proportion of TiH2 powder and B powder was calculated based on the molar ratio of Ti atoms to B atoms of 1:2, and the content of in-situ generated TiB2 particles accounted for 1wt.%-5wt.% of the Cu+TiH2+B precursor powder. Cu powder, TiH2 powder and B powder were weighed respectively, and then the three raw material powders were inverted into the same ball mill at the same time. The ball mill beads were weighed according to the mass of the powder in the ball mill at a ball-to-material ratio of 10:1-20:

1. Anhydrous ethanol was added as a process control agent according to 1wt.%-3wt.% of the mass of the powder in the ball mill, and then the ball mill was evacuated to 1.0×10 -2 Pa, and then fill with argon gas to a low negative pressure, repeating this process several times to ensure that the ball mill is completely protected by an argon atmosphere; finally, the ball mill is placed in a ball mill for a ball milling process at a speed of 350r / min-450r / min and a ball milling time of 5h-20h to obtain a spherical Cu+TiH2+B precursor powder; In step 1, the particle size of the spherical Cu+TiH2+B precursor powder ranges from 200 to 900 μm; Step 2: Mix the spherical Cu+TiH2+B precursor powder and pure Cu powder in proportion by using a vibration powder mixing device; In step 2, the spherical Cu+TiH2+B precursor powder and the pure Cu powder are subjected to three-dimensional vibration mixing at a mass ratio of 4:1-1:4 to obtain a mixed powder of the spherical Cu+TiH2+B precursor powder and the pure Cu powder, wherein the frequency of the vibration mixing is 30Hz-50Hz, and the vibration time is 1h-3h; Step 3: cold pressing the mixed powder mixed thoroughly in step 2 to obtain a cold pressed blank; The specific implementation of step 3 is: Weigh the mixed powder obtained in step 2 and place it in a quenched steel cold pressing mold, and perform cold pressing molding on it with a loading pressure of 50MPa-200MPa and a holding time of 40s-60s by a four-column hydraulic press to obtain a cold pressed blank with a higher density; Step 4: placing the compact in a graphite mold for hot pressing and sintering to prepare an isolated island structure TiB2 / Cu-Cu composite material; The specific implementation of step 4 is: The cold pressed blank is loaded into a graphite crucible and placed in the center of a sintering furnace. The cover of the hot pressing furnace is closed for sintering. The sintering atmosphere is inert gas protection or vacuum. The sintering process is first heated to 850°C-900°C at a rate of 10°C / min-30°C / min and kept warm for 0.5h-1h, then continued to heat to 950°C-1050°C and kept warm for 0.5h-2h at a pressure of 0MPa-50MPa, and then cooled to room temperature with the furnace to obtain an isolated island structure TiB2 / Cu-Cu composite material.

2. Isolated island structure TiB2 / Cu-Cu composite material, characterized in that: The method according to claim 1 is used to prepare it.

Citation Information

Patent Citations

  • Method for preparing high-conductivity titanium diboride / copper composite material

    CN107586988A

  • Three-dimensional net structured titanium diboride reinforced copper base composite material and preparation method thereof

    CN107675009A

  • In-situ synthesized titanium boride reinforced copper-based composite material, and preparation method and application thereof

    CN108085534A

  • Nonuniform structure titanium diboride / copper composite and preparation method thereof

    CN108251681A

  • Post-treatment method for hot-pressing sintered titanium diboride reinforced copper-based composite

    CN110358990A