A high-strength heat-resistant rare earth magnesium alloy and preparation method thereof
By adding Nd to magnesium alloys and using a multi-stage variable-temperature forging process, the problem of strength reduction in magnesium alloys at high temperatures was solved, resulting in high-performance, large-size forgings suitable for aerospace and military applications.
Patent Information
- Application Number
- CN202211605097.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-14
AI Technical Summary
Existing high-strength heat-resistant magnesium alloys exhibit significant strength reduction at high temperatures, failing to meet the high-temperature requirements of industries such as aerospace, military, and automotive. Furthermore, large load-bearing components suffer from casting defects and poor forging deformation capabilities.
By adding 0.1-0.5% of Nd trace elements, a high-temperature stable phase -Mg12Nd is formed. Combined with a multi-fire, multi-temperature, multi-directional forging process, the grain structure is refined, and the high-temperature mechanical properties of the alloy are improved.
Excellent mechanical properties of the alloy at high temperatures were achieved, material costs were reduced, and a fine and uniform grain structure was obtained, making it suitable for the aerospace field.
Smart Images

Figure CN115927939B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of magnesium alloy metal materials, and in particular to a high-strength heat-resistant rare earth magnesium alloy and a preparation method thereof. Background Art
[0002] With the development of aerospace industry, the country's demand for lightweight materials is increasing. As the lightest structural material, magnesium alloy has unique advantages. Rare earth magnesium alloy is known as high-strength and high-temperature resistant magnesium alloy. The material cost is high. In order to ensure the comprehensive performance and maximum weight reduction effect in high-temperature service environment, a large number of weapon systems usually use high-temperature heat-resistant magnesium alloy as the first choice. Mg-Y and Mg-Gd are currently the best magnesium alloys in high-temperature mechanical properties, creep resistance and heat resistance. However, the main shortcomings of existing commercial high-strength heat-resistant magnesium alloys such as WE54, VW83M, VW93M, etc. are that although the mechanical properties are high at room temperature, the strength decreases significantly at high temperature, and it cannot fully meet the higher strength requirements when used at high temperatures in aerospace, military, automotive and other industries.
[0003] At present, most rare earth magnesium alloy products are die-castings. Inclusions, pores and other defects in cast magnesium alloys will significantly reduce the mechanical properties of the alloy. Therefore, they cannot be matched and applied to large load-bearing parts with high mechanical performance requirements, such as weapons and missile hulls. There are also few applications of high-performance large-size forgings. The main reason is that the crystal structure of magnesium alloys is hexagonal close-packed, there are fewer slip systems that can be activated at room temperature, and the forging deformation ability is poor, which leads to the problem of easy cracking of large-size forgings during the forging process.
[0004] Chinese patent CN107090558A discloses a high-strength heat-resistant cast magnesium alloy, whose mass percentages are: Gd 6-13%, Y 2-6%, Zr 0.3-0.8%, Ca 0.3-0.6%, Si ≤0.01%, cerium-rich mixed rare earth 0.7-3.0%, and the rest is Mg, but its maximum tensile strength at room temperature is only about 370Mpa, which does not meet the performance requirements of high-load-bearing parts above 400Mpa, and the comprehensive rare earth content is relatively high, about 20%, resulting in high material preparation costs and is not conducive to promotion and application.
[0005] Chinese patent CN109666832A relates to a high-strength heat-resistant deformable magnesium alloy and its preparation method, the alloy composition is 7.0-9.0wt% Gd, >0 and ≤4.0wt% Yb, 1.0-1.5wt% Zn, 0.4-0.6wt% Zr, the balance is Mg and inevitable impurity elements. However, the yield strength of the magnesium alloy at 250°C can only be maintained at about 300MPa, which cannot well meet the use requirements of load-bearing structural parts with high service temperature.
[0006] Therefore, the current research focus is to rationally regulate the content of each element in the rare earth magnesium alloy so that it has good room temperature and high temperature mechanical properties while controlling the material cost. At the same time, by designing the forging process deformation temperature, deformation rate and other parameters, its plastic deformation ability can be significantly improved to obtain high-performance forgings. Summary of the invention
[0007] In order to solve the above technical problems, the purpose of the present invention is to provide a high-strength and heat-resistant rare earth magnesium alloy and a preparation method thereof to meet the production of large-size and high-performance rare earth magnesium alloy forgings.
[0008] In order to meet the above objectives, the present invention adopts the following technical solution: a high-strength and heat-resistant rare earth magnesium alloy, which is composed of elements such as Mg, Gd, Y, Zr, and Nd, and the mass percentage of each component is: Gd: 8.5-10.0%, Y: 2.5-4.0%, Zr: 0.3-0.8%, Nd: 0.1-0.5%, the sum of Gd content and Y content is: 11.5≤Gd+Y≤13.5, and the balance is magnesium and other inevitable impurity elements.
[0009] Research has found that after adding trace amounts of Nd to magnesium alloys, after solution and aging treatment, part of the Nd element remains dissolved in the magnesium matrix, strengthening the matrix and hindering the slip of dislocations, thereby increasing the deformation resistance of the matrix; while the other part combines with Mg to form a high-temperature stable intermetallic compound - Mg 12 Nd is uniformly dispersed and precipitated near the grain boundary, effectively inhibiting the grain boundary movement, thereby improving the high temperature mechanical properties of the alloy. Therefore, in the present invention, by adding 0.1-0.5% Nd trace element, a high temperature stable phase - Mg is formed in the alloy. 12 Nd is added to improve the high temperature mechanical properties of the alloy; then a multi-fire variable temperature forging deformation process is adopted to obtain large-sized forgings with fine and uniform grain structure and good plastic deformation ability. The final forgings have excellent room temperature (25℃) and high temperature (250℃) mechanical properties.
[0010] The present invention also provides a method for preparing the high-strength heat-resistant rare earth magnesium alloy, comprising the following steps:
[0011] 1) Semi-continuous casting: Add the raw materials with good proportions into the smelting furnace in order. After smelting, use a crane to take out the cast bars;
[0012] 2) Homogenization heat treatment: The magnesium alloy ingot obtained in step 1) is subjected to homogenization heat treatment, and the temperature control homogenization heat treatment system is: 460-500°C, the heating rate is 4-7°C / min, and after reaching the set temperature, the temperature is kept for 12-36 hours, and air-cooled;
[0013] 3) Multi-fire variable temperature multi-directional forging: subjecting the magnesium alloy obtained in step 2) to a homogenized heat-treated magnesium alloy ingot to variable temperature multi-directional forging to obtain a forged magnesium alloy part, wherein the multi-directional forging is variable temperature two-fire forging;
[0014] The first fire forging process is:
[0015] a) The cast bars are heated in the furnace, with the holding temperature at 480-500°C and the holding time at 8-12h;
[0016] b) Preheat the upper and lower forging plates to 400-500℃;
[0017] c) Free forging is performed, and direction reversal is required during each upsetting process. The number of upsetting reversals is 1-3 times, the first upsetting reduction is 50%-60%, the other upsetting single-pass reduction is 30%-50%, the single-pass reduction is 10%-20%, the total forging passes are ≥30 passes, the pressing speed is 5-15mm / s, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging after each reversal, and the billet height-to-diameter ratio is 1.5-3.0 after each reversal;
[0018] The second fire forging process is:
[0019] a) Return to the furnace for heat preservation at a temperature of 460-480°C for 1-4h;
[0020] b) Preheat the upper and lower forging plates to 400-480℃;
[0021] c) Free forging is performed, and direction reversal is required during each upsetting and drawing process. The number of upsetting and drawing reversals is 1-3 times, the first upsetting reduction is 50%-60%, the other upsetting single-pass reduction is 30%-50%, the single-pass reduction is 10%-20%, the total forging passes are ≥30 passes, the pressing speed is 5-15mm / s, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging after each reversal, the billet height-to-diameter ratio is 1.5-3.0 after each reversal, and the upsetting and drawing is the required forging size after the last reversal forging;
[0022] 4) Aging heat treatment: The forging obtained in step 3) is subjected to aging heat treatment, and then naturally cooled to room temperature to obtain the high-strength and heat-resistant rare earth magnesium alloy. The aging heat treatment temperature is 180-240° C., and the time is 12-30 hours.
[0023] The existing commercial high-strength heat-resistant magnesium alloys have high mechanical properties at room temperature, but the strength drops significantly at high temperatures, and cannot fully meet the higher strength requirements for use at high temperatures in aerospace, military, automotive and other industries. Currently, most rare earth magnesium alloy products are die-castings, but the presence of defects such as inclusions and pores in cast magnesium alloys will significantly reduce the mechanical properties of the alloy. Therefore, they cannot be matched and applied in certain large load-bearing parts with high mechanical property requirements, such as weapons and missile hulls. There are also few applications for high-performance large-size forgings. The main reason is that the crystal structure of magnesium alloys is hexagonal close-packed, there are fewer slip systems that can be activated at room temperature, and the forging deformation ability is poor, resulting in the problem of easy cracking of large-size forgings during the forging process.
[0024] Compared with the prior art, the advantages of the present invention are:
[0025] The present invention forms a high temperature stable phase -Mg in the alloy by adding 0.1-0.5% Nd trace element 12 Nd improves the high temperature mechanical properties of the alloy, and adopts multi-fire temperature-changing forging to obtain large-sized forgings with fine and uniform grain structure and good plastic deformation ability. The forgings have excellent mechanical properties at room temperature (25℃) and high temperature (250℃), and can be promoted and applied in the aerospace field. The specific advantages are as follows:
[0026] (1) The present invention forms a high temperature stable phase -Mg in the alloy by adding 0.1-0.5% Nd trace element 12 Nd improves the high temperature mechanical properties of the alloy.
[0027] (2) By adding 0.1-0.5% Nd trace element, the total content of rare earth elements and precious metal elements (such as Y and Ag) in the present invention is lower than that of existing commercial high-strength and heat-resistant magnesium alloys, thereby reducing material costs and being applicable in the aerospace field.
[0028] (3) The present invention adopts a new multi-fire variable temperature multi-directional forging process. Compared with the traditional isothermal multi-directional forging process, it further refines the grain structure of the workpiece and obtains large-sized forgings with equiaxed grains and good plastic deformation ability. The forgings have excellent mechanical properties at room temperature (25°C) and high temperature (250°C). The room temperature tensile strength reaches more than 450MPa, and the yield strength reaches more than 370MPa; the high temperature tensile strength reaches more than 320MPa, and the yield strength reaches more than 230MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Attached Figure 1 is an optical microstructure metallographic image of the alloy in the forged state in Example 1 of the present invention;
[0030] Attached Figure 2 This is a diagram of the forging billet of the alloy in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0032] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0033] In the whole text of the present invention, unless otherwise specified, the content of each component is percentage by weight, and the ratio of each component is percentage by weight.
[0034] Embodiment 1:
[0035] A high-strength heat-resistant rare earth magnesium alloy of the present invention comprises the following components in percentage by mass:
[0036] Gd: 9.28%, Y: 2.83%, Zr: 0.34%, Nd: 0.43%, and the balance is Mg and other inevitable impurity elements.
[0037] The method for preparing the high-strength heat-resistant rare earth magnesium alloy of this embodiment comprises the following steps:
[0038] 1) Semi-continuous casting: Add the raw materials with good proportions into the smelting furnace in sequence. After smelting, use a crane to take out the cast rods.
[0039] 2) Homogenization heat treatment: The magnesium alloy ingot obtained in step 1) is subjected to homogenization heat treatment, and the homogenization heat treatment is controlled as follows: target temperature 490°C, heating rate 5°C / min, and after reaching the set temperature, the temperature is kept for 24 hours and air-cooled.
[0040] 3) Multi-fire multi-directional forging with variable temperature: The magnesium alloy ingot obtained in step 2) after homogenization heat treatment is subjected to variable temperature multi-directional forging to obtain a forged magnesium alloy part, wherein the multi-directional forging is two-fire forging.
[0041] The first fire forging process is:
[0042] a) The cast rods are heated in a furnace at a holding temperature of 500°C for 8 hours.
[0043] b) Preheat the upper and lower forging plates to 450℃.
[0044] c) Free forging is performed. Reversal is required during each upsetting and drawing process. The number of reversals is 3. The first upsetting reduction is 53%, the remaining upsetting reductions are 45%, and the drawing reduction is 15%. The total forging is 36 passes. The pressing speed is 10 mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.5.
[0045] The second fire forging process is:
[0046] a) Return to the furnace and keep warm at 470℃ for 3h.
[0047] b) Preheat the upper and lower forging plates to 440℃.
[0048] c) Free forging is performed. Direction reversal is required during each upsetting and drawing process. The number of upsetting and drawing reversals is 3 times. The first upsetting reduction is 53%, the remaining upsetting reductions are 45%, and the drawing reduction is 15%. The total forging is 36 times. The pressing speed is 10mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.5. After the last reversal forging, the upsetting and drawing is the required forging size.
[0049] 4) Aging heat treatment: The forged magnesium alloy part obtained in step 3) is subjected to aging heat treatment to obtain an aging heat treated magnesium alloy forging, and the aging heat treated magnesium alloy forging is naturally cooled to room temperature to obtain a high-strength and heat-resistant rare earth magnesium alloy. The aging heat treatment temperature is 220°C and the time is 24 hours.
[0050] The metallographic photographs of the alloy forgings are as follows: Figure 1 As shown in the figure, the grain structure of the forging is fine, most of which are equiaxed grains, the smallest grain is only about 5-7μm, the largest grain is about 103-114μm, the average grain size is about 30μm, and most grains are between 5-50μm. This shows that after forging, the grains are effectively refined. According to the Hall-Page formula:
[0051] σ5=σ0+Kd -1 / 2
[0052] The strength of the alloy is inversely proportional to the grain size, and the finer the grain, the higher the strength. Therefore, after the billet passes through the end, the internal deformation of the magnesium alloy is relatively sufficient, the grain is refined, the mechanical properties are improved, and the mechanical properties of the forging are good.
[0053] The appearance of the alloy forging blank is as follows Figure 2 As shown in the figure, it can be seen that the surface quality of the forging is good and no cracks appear, which shows that the forging has good formability and the forging process parameters are appropriate.
[0054] Embodiment 2:
[0055] A high-strength heat-resistant rare earth magnesium alloy of the present invention comprises the following components in percentage by mass:
[0056] Gd: 9.41%, Y: 2.52%, Zr: 0.43%, Nd: 0.38%, and the balance is Mg and other inevitable impurity elements.
[0057] The method for preparing the high-strength heat-resistant rare earth magnesium alloy of this embodiment comprises the following steps:
[0058] 1) Semi-continuous casting: Add the raw materials with good proportions into the smelting furnace in sequence. After smelting, use a crane to take out the cast rods.
[0059] 2) Homogenization heat treatment: The magnesium alloy ingot obtained in step 1) is subjected to homogenization heat treatment, and the homogenization heat treatment is controlled as follows: target temperature 500°C, heating rate 5°C / min, and after reaching the set temperature, the temperature is kept for 16 hours and air-cooled.
[0060] 3) Multi-fire multi-directional forging with variable temperature: The magnesium alloy ingot obtained in step 2) after homogenization heat treatment is subjected to variable temperature multi-directional forging to obtain a forged magnesium alloy part, wherein the multi-directional forging is two-fire forging.
[0061] The first fire forging process is:
[0062] a) The cast rods are heated in a furnace at a holding temperature of 480°C for 12 hours.
[0063] b) Preheat the upper and lower forging plates to 450℃.
[0064] c) Free forging is performed. Reversal is required during each upsetting and drawing process. The number of reversals is 3. The first upsetting reduction is 55%, the remaining upsetting reductions are 40%, the drawing reductions are 20%, the total forging is 33 passes, the pressing speed is 10 mm / s, and after each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.0.
[0065] The second fire forging process is:
[0066] a) Return to the furnace and keep warm at 460℃ for 4h.
[0067] b) Preheat the upper and lower forging plates to 440℃.
[0068] c) Free forging is performed. Direction reversal is required during each upsetting and drawing process. The number of upsetting and drawing reversals is 3 times. The first upsetting reduction is 55%, the remaining upsetting reductions are 40%, and the drawing reductions are 20%. The total forging is 33 times. The pressing speed is 10 mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.0. After the last reversal forging, the upsetting and drawing is the required forging size.
[0069] 4) Aging heat treatment: The forged magnesium alloy part obtained in step 3) is subjected to aging heat treatment to obtain an aging heat treated magnesium alloy forging, and the aging heat treated magnesium alloy forging is naturally cooled to room temperature to obtain a high-strength and heat-resistant rare earth magnesium alloy. The aging heat treatment temperature is 240°C and the time is 18 hours.
[0070] Embodiment 3:
[0071] A high-strength heat-resistant rare earth magnesium alloy of the present invention comprises the following components in percentage by mass:
[0072] Gd: 8.9%, Y: 3.01%, Zr: 0.33%, Nd: 0.40%, and the balance is Mg and other inevitable impurity elements.
[0073] The method for preparing the high-strength heat-resistant rare earth magnesium alloy of this embodiment comprises the following steps:
[0074] 1) Semi-continuous casting: Add the raw materials with good proportions into the smelting furnace in sequence. After smelting, use a crane to take out the cast rods.
[0075] 2) Homogenization heat treatment: The magnesium alloy ingot obtained in step 1) is subjected to homogenization heat treatment, and the homogenization heat treatment is controlled as follows: target temperature 480°C, heating rate 5°C / min, and after reaching the set temperature, the temperature is kept for 30 hours and air-cooled.
[0076] 3) Multi-fire multi-directional forging with variable temperature: The magnesium alloy ingot obtained in step 2) after homogenization heat treatment is subjected to variable temperature multi-directional forging to obtain a forged magnesium alloy part, wherein the multi-directional forging is two-fire forging.
[0077] The first fire forging process is:
[0078] a) The cast rods are heated in a furnace at a holding temperature of 490°C for 12 hours.
[0079] b) Preheat the upper and lower forging plates to 450℃.
[0080] c) Free forging is performed. Direction reversal is required during each upsetting and drawing process. The number of reversals is 3. The first upsetting reduction is 58%, the remaining upsetting reductions are 42%, and the drawing reduction is 18%. The total forging is 34 passes. The pressing speed is 10 mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.5.
[0081] The second fire forging process is:
[0082] a) Return to the furnace and keep warm at 480℃ for 2h.
[0083] b) Preheat the upper and lower forging plates to 440℃.
[0084] c) Free forging is performed. Direction reversal is required during each upsetting and drawing process. The number of upsetting and drawing reversals is 3 times. The first upsetting reduction is 58%, the remaining upsetting reductions are 42%, and the drawing reduction is 18%. The total forging is 34 times. The pressing speed is 10mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.5. After the last reversal forging, the upsetting and drawing is the required forging size.
[0085] 4) Aging heat treatment: The forged magnesium alloy part obtained in step 3) is subjected to aging heat treatment to obtain an aging heat treated magnesium alloy forging, and the aging heat treated magnesium alloy forging is naturally cooled to room temperature to obtain a high-strength and heat-resistant rare earth magnesium alloy. The aging heat treatment temperature is 190°C and the time is 30 hours.
[0086] Comparative Example 1:
[0087] A magnesium alloy comprising the following components in percentage by mass:
[0088] Gd: 8.89%, Y: 3.0%, Zr: 0.34%, and the balance is Mg and other inevitable impurity elements.
[0089] The preparation method of the magnesium alloy of this comparative example comprises the following steps:
[0090] 1) Semi-continuous casting: Add the raw materials with good proportions into the smelting furnace in sequence. After smelting, use a crane to take out the cast rods.
[0091] 2) Homogenization heat treatment: The magnesium alloy ingot obtained in step 1) is subjected to homogenization heat treatment, and the homogenization heat treatment is controlled as follows: target temperature 480°C, heating rate 5°C / min, and after reaching the set temperature, the temperature is kept for 30 hours and air-cooled.
[0092] 3) Multi-fire multi-directional forging with variable temperature: The magnesium alloy ingot obtained in step 2) after homogenization heat treatment is subjected to variable temperature multi-directional forging to obtain a forged magnesium alloy part, wherein the multi-directional forging is two-fire forging.
[0093] The first fire forging process is:
[0094] a) The cast rods are heated in a furnace at a holding temperature of 490°C for 12 hours.
[0095] b) Preheat the upper and lower forging plates to 450℃.
[0096] c) Free forging is performed. Direction reversal is required during each upsetting and drawing process. The number of reversals is 3. The first upsetting reduction is 58%, the remaining upsetting reductions are 42%, and the drawing reduction is 18%. The total forging is 34 passes. The pressing speed is 10 mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.5.
[0097] The second fire forging process is:
[0098] a) Return to the furnace and keep warm at 480℃ for 2h.
[0099] b) Preheat the upper and lower forging plates to 440℃.
[0100] c) Free forging is performed. Direction reversal is required during each upsetting and drawing process. The number of upsetting and drawing reversals is 3 times. The first upsetting reduction is 58%, the remaining upsetting reductions are 42%, and the drawing reduction is 18%. The total forging is 34 times. The pressing speed is 10mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the billet height-to-diameter ratio is 2.5. After the last reversal forging, the upsetting and drawing is the required forging size.
[0101] 4) Aging heat treatment: The forged magnesium alloy part obtained in step 3) is subjected to aging heat treatment to obtain an aging heat treated magnesium alloy forging, and the aging heat treated magnesium alloy forging is naturally cooled to room temperature to obtain a magnesium alloy. The aging heat treatment temperature is 190° C. and the time is 30 hours.
[0102] Comparative Example 2:
[0103] A magnesium alloy of the present invention comprises the following components in percentage by mass:
[0104] Gd: 8.91%, Y: 3.02%, Zr: 0.35%, Nd: 0.41%, and the balance is Mg and other inevitable impurity elements.
[0105] The preparation method of the magnesium alloy of this comparative example comprises the following steps:
[0106] 1) Semi-continuous casting: Add the raw materials with good proportions into the smelting furnace in sequence. After smelting, use a crane to take out the cast rods.
[0107] 2) Homogenization heat treatment: The magnesium alloy ingot obtained in step 1) is subjected to homogenization heat treatment, and the homogenization heat treatment is controlled to a target temperature of 480°C, a heating rate of 5°C / min, and after reaching the set temperature, the temperature is kept for 30 hours and air-cooled.
[0108] 3) Multi-directional forging: Preheat the magnesium alloy ingot in a medium frequency furnace. The temperature of the medium frequency furnace is set to 490℃ and kept warm for 12 hours. The upper and lower forging anvils are preheated to 450℃. The forging temperature is 480℃. The number of reversals of upsetting and drawing is 3 times. The downstroke amount of upsetting is 40%, and the downstroke amount of drawing is 20%. The total forging is 30 times. The downstroke speed is 10mm / s. After each reversal, the axial direction of the forging blank is perpendicular to the axial direction of the ingot before forging. After each reversal, the aspect ratio of the blank is 2.5. After the last reversal forging, the upsetting and drawing are the required forging size.
[0109] 4) Aging heat treatment: The forged magnesium alloy part obtained in step 3) is subjected to aging heat treatment to obtain an aging heat treated magnesium alloy forging, and the aging heat treated magnesium alloy forging is naturally cooled to room temperature to obtain a magnesium alloy. The aging heat treatment temperature is 190° C. and the time is 30 hours.
[0110] Table 1 Room temperature mechanical properties of high strength and heat resistant rare earth magnesium alloys in Examples 1-3
[0111]
[0112] Table 2 Room temperature mechanical properties of magnesium alloys in comparative examples 1-2
[0113]
[0114] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. Therefore, the scope of protection of the present invention should be subject to the scope of protection of the claims.
Claims
1. A method for preparing a high-strength heat-resistant rare earth magnesium alloy, characterized in that: The following components are included in mass percentage: Gd: 8.5-10.0%; Y:2.5-4.0%; Zr:0.3~0.8%; Nd: 0.1-0.38%; The sum of Gd content and Y content is: 11.5≤Gd+Y≤13.5%; The balance is magnesium and other unavoidable impurity elements; The preparation method comprises the following steps: Step S1: smelting various raw materials to obtain a magnesium alloy melt, and then performing semi-continuous casting to obtain a magnesium alloy ingot; Step S2: performing homogenization heat treatment on the magnesium alloy ingot to obtain a homogenization heat treated magnesium alloy ingot; Step S3: subjecting the magnesium alloy ingot after homogenization heat treatment to variable temperature multi-directional forging to obtain a forged magnesium alloy part; Step S4: subjecting the forged magnesium alloy part to aging heat treatment to obtain an aging heat treated magnesium alloy forging, and naturally cooling the aging heat treated magnesium alloy forging to room temperature to obtain the high-strength and heat-resistant rare earth magnesium alloy; The variable temperature multi-directional forging in step S3 includes variable temperature two-fire forging: the magnesium alloy ingot is returned to the furnace for the second fire forging after the first fire forging, and the furnace temperature and the holding time of the first fire forging are higher than the furnace temperature and the holding time of the second fire forging; The first fire forging process comprises the following steps: The magnesium alloy ingot is heated in a furnace, the holding temperature is 480-500℃, the holding time is 8-12h, and then free forging is performed. The direction is changed during each upsetting process, and the number of upsetting and drawing direction changes is 1-3 times. The first upsetting reduction is 50%-60%, the other upsetting single-pass reduction is 30%-50%, and the single-pass reduction of the drawing is 10%-20%. The total forging passes are ≥30 passes, and the pressing speed is 5-15mm / s. After each reversal, the axial direction of the forging billet is perpendicular to the axial direction of the ingot before forging, and the billet height-to-diameter ratio after each reversal is 1.5-3.0; Before the free forging, the upper and lower forging anvils are preheated to 400-500°C; The process of the second fire forging is: The magnesium alloy ingot after the first forging is returned to the furnace for insulation at a temperature of 460-480°C for a time of 1-4 hours; free forging is performed, and the free forging method and process parameters are the same as the free forging in the first forging process, and after the last reversing forging, the ingot is upset and drawn to the required forging size.
2. The method for preparing a high-strength heat-resistant rare earth magnesium alloy according to claim 1, characterized in that: The homogenization heat treatment in step S2 is specifically as follows: heating from room temperature to 460-500°C at a heating rate of 4-7°C / min, maintaining the temperature for 12-36 hours after reaching the set temperature, and then cooling to room temperature in air.
3. The method for preparing a high-strength heat-resistant rare earth magnesium alloy according to claim 1, characterized in that: Before the second free forging, the upper and lower forging anvils are preheated to 400-480°C.
4. The method for preparing a high-strength heat-resistant rare earth magnesium alloy according to claim 1, characterized in that: The temperature of the aging heat treatment in step S4 is 180-240° C. and the time is 12-30 hours.
Citation Information
Cited By
Method for improving creep resistance of rare earth magnesium alloy
CN121737494A