A bio-based oligomer remover and its preparation method and application
Through the use of bio-based oligomer removers, the problem of incomplete removal of oligomers in the existing technology is solved, the dyeing effect and equipment cleanliness are improved, and the dyeing quality and environmental protection performance of textiles are significantly improved.
Patent Information
- Application Number
- CN202310010558.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-01-04
AI Technical Summary
Existing oligomer removers cannot completely remove oligomers from fabrics, resulting in color bars, color spots and 'white powder' phenomena during the dyeing process, affecting the dyeing effect and equipment cleanliness.
Bio-based oligomer remover is used, including bio-based organic fatty acids, alcohol polymers, catalysts, natural grease sulfonated oils and solvents, and is prepared through specific ratios and process steps to form a non-ionic surfactant and anionic High-temperature oligomer remover that works synergistically with surfactants to improve dyeing results and equipment cleanliness.
It achieves consistent color depth on the surface of the dyed cloth, avoids color stripes, color spots and 'white powder' phenomena, improves the leveling performance of the dye and the cleanliness of the fabric, and significantly improves product quality and environmental performance.
Smart Images

Figure BSA0000293078830000021 
Figure BSA0000293078830000041 
Figure BSA0000293078830000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile printing and dyeing in the printing and dyeing production of the textile industry, and in particular relates to a bio-based oligomer remover and a preparation method and application thereof. Background Art
[0002] Petroleum-based products are textile auxiliaries made by refining and synthesizing petroleum as raw materials. Many of these textile auxiliaries contain or produce chemical substances that are harmful to human health and the ecological environment during use. Toxic and harmful substances remaining on textiles and clothing also directly affect human health and safety. In recent years, the more serious thing is that the traditional petrochemical economy based on petroleum has paid a huge environmental price, such as sewage discharge, air pollution, white pollution, greenhouse effect, etc., which has aroused people's widespread concern and thinking about the source of power for future social development.
[0003] Bio-based products have good biodegradability and are environmentally friendly. They can reduce the use of traditional petroleum-based chemicals, have low production costs, significant economic benefits, and clean production, which helps protect the ecological environment. With the enhancement of people's environmental awareness and the improvement of national environmental protection laws and regulations, the textile printing and dyeing industry needs to develop in the direction of biomass to achieve green and sustainable development of the industry.
[0004] Oligomers, also known as oligomers, oligomers, and short polymers, are low molecular weight substances with the same chemical structure as polyester fibers that exist inside polyester fibers. They are by-products in the polyester spinning process. Generally, polyester contains 1-3% oligomers. Oligomers are polymers composed of fewer repeating units, and their relative molecular mass is between small molecules and macromolecules. Most polyester oligomers are cyclic compounds formed by three ethyl terephthalates. When the temperature exceeds 120°C, oligomers can dissolve in the dye bath and crystallize from the solution and combine with the condensed dye. When cooled, they are deposited on the surface of the machine or fabric to form defects such as color spots and color dots. Disperse dyeing generally requires keeping the temperature at 130°C for about 30 minutes to ensure the depth and fastness of the dyeing. Therefore, adding a special oligomer remover during dyeing can be used for prevention. It can prevent oligomer (white powder) contamination of polyester during the dyeing process, which can not only produce a level dyeing effect, but also prevent oligomers from precipitating on the fabric; when used for cheese dyeing, it can reduce the layer difference caused by oligomers, effectively eliminate the "white powder" phenomenon, make the yarn cleaner, facilitate winding, and improve the level dyeing performance of disperse dyes. At the same time, after multiple dyeing, it is also necessary to use oligomer removers to clean the equipment to maintain the cleanliness of the dyeing tank and prevent secondary contamination of residual oligomers. Oligomer removers are indispensable additives in high-temperature dyeing of polyester.
[0005] Currently, most oligomer removers used in the market are anionic surfactants, and their oligomer removal abilities vary, but none of them can completely and thoroughly remove oligomers from fabrics. Summary of the invention
[0006] The purpose of the present invention is to provide a bio-based oligomer remover and a preparation method and application thereof. After dyeing with the oligomer remover provided by the present invention, the color depth, color light and brightness of the cloth surface are consistent, and no defects such as color stripes, color spots, and "white powder" are generated.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] A bio-based oligomer remover, the raw materials of which include bio-based organic fatty acid, alcohol polymer, catalyst, natural fat sulfonated oil and solvent;
[0009] Taking the total mass of the raw materials of the oligomer remover as 100%, the mass percentage of each component is:
[0010]
[0011] The bio-based organic fatty acids are bio-based tall oil fatty acids and bio-based heneicosadicarboxylic acid;
[0012] The alcohol polymer is at least one of polyethylene glycol PEG400, PEG-600, and PEG-800;
[0013] The catalyst is p-toluenesulfonic acid;
[0014] The natural sulphonated oil is at least one of natural sulphonated rapeseed oil, natural sulphonated castor oil and sulphated natural neatsfoot oil;
[0015] The solvent is at least one of diethylene glycol butyl ether, dipropylene glycol methyl ether and ethanol;
[0016] The natural oil sulfonated oil is added in an amount of 20%-30%. Within this range, the stability of the oligomer remover and high temperature dyeing will not be significantly affected;
[0017] The alcohol polymer is selected to be 30%-40%. When the alcohol polymer is less than 25%, the esterification of the bio-based organic fatty acid is incomplete, affecting the leveling effect; when the alcohol polymer is greater than 50%, explosion is likely to occur during the reaction;
[0018] The catalyst is 0.1%-1%. When the catalyst is less than 0.1%, the reaction speed is slow, the heating and heat preservation time is prolonged, and implosion is likely to occur; when the catalyst is greater than 2%, the reaction speed is too fast and difficult to control, and implosion is likely to occur during the reaction;
[0019] In the present invention, the oligomer remover further comprises the following components in parts by weight:
[0020] Oxidant 0.1%-2%
[0021] Defoamer 0.01%-1%
[0022] The oxidant is 0.1%-2%, such as 0.1%, 0.2%, 0.3%;
[0023] The oxidant is hypophosphorous acid H3PO2, which has strong oxidizing properties and can assist with the catalyst to make the initiation efficiency higher;
[0024] The defoaming agent is used in an amount of 0.01%-1%, such as 0.01%, 0.1%, 0.5%;
[0025] The defoaming agent is at least one of silicone, polyether, and polyether-modified polysiloxane, preferably polyether-modified polysiloxane, which can quickly penetrate into the foam in a high-temperature foaming system to destroy the stability of the foam, thereby achieving a defoaming effect;
[0026] A method for preparing a bio-based oligomer remover comprises the following steps:
[0027] Step 1: Adding bio-based organic fatty acid into a reactor and stirring;
[0028] Step 2: Add the alcohol polymer into the reactor of step 1 and stir;
[0029] Step 3, adding the oxidant into the reactor of step 2 and stirring;
[0030] Step 4: Add the catalyst into the reactor of step 3 and stir;
[0031] Step 5: Stir the materials evenly, and start heating to 150-155°C to melt;
[0032] Step 6: Continue to heat up to 235-240°C to carry out dehydration reaction;
[0033] Step 7, cooling to 180-190°C, and continuing the dehydration reaction;
[0034] Step 8: After the dehydration reaction is completed, the temperature is naturally lowered to below 45°C;
[0035] Step 9, add natural fat sulfonated oil and stir;
[0036] Step 10, adding solvent and stirring;
[0037] Step 11: Add defoaming agent and stir to obtain oligomer remover.
[0038] Preferably, in step 1, the stirring speed is 20-30 rpm, the temperature does not exceed 35° C., and nitrogen is introduced for protection;
[0039] Preferably, in step 5, stirring is maintained for 20-30 min, and nitrogen protection is introduced;
[0040] Preferably, in step six, the stirring speed is 55-65 rpm, the reaction time is 1-3 h, and nitrogen protection is introduced;
[0041] Preferably, in step 7, after cooling to 180-190°C, the nitrogen is turned off, vacuum is drawn, and the reaction time is 20-30 minutes;
[0042] Preferably, in step eight, after the dehydration reaction is completed, vacuum is first evacuated, nitrogen is introduced, and then the temperature is naturally lowered to below 45° C.;
[0043] Preferably, in step nine, the stirring speed is 20-30 rpm, and the stirring is 50-60 min;
[0044] Preferably, in step 10, the stirring speed is 20-30 rpm and the stirring time is 10-20 min.
[0045] Preferably, in step eleven, the stirring speed is 20-30 rpm, and the stirring is performed for 10-20 min.
[0046] An application of a bio-based oligomer remover, in which the environmentally friendly disperse dye high-temperature dyeing process is used, the dye liquor ratio is:
[0047]
[0048] The composition and proportion of the reduction cleaning fluid used are:
[0049] Alkali 0.1%-1%
[0050] Reducing agent 0.1%-1%
[0051] Oligomer remover 0.1%-2%
[0052] The above ingredients are added with excess water to form a dye solution, and the polyester high-temperature dyeing process is carried out. The polyester high-temperature dyeing process is as follows: the prepared dye solution is poured into a dye cup, and a polyester standard cloth is added. The temperature is raised to 130-135°C, and after keeping the temperature for 40-50 minutes, the temperature is lowered to below 50°C, and the dye solution is drained. The dye solution is then treated with a reducing cleaning solution containing an oligomer remover at 75-85°C for 10-20 minutes and then discharged. The dyed cloth is washed with hot water, washed with cold water, washed with acid, washed with cold water, and dried in turn. Subsequently, the leveling performance and migration performance of the polyester standard cloth during the dyeing process are evaluated.
[0053] The environmentally friendly disperse dye red is KELISOL ACE series of Xinruibei Company: red AC-E;
[0054] The environmentally friendly disperse dye yellow is KELISOL ACE series of Xinruibei Company: Yellow AC-E;
[0055] The environmentally friendly disperse dye blue is KELISOL ACE series of Xinruibei Company: blue AC-E;
[0056] The pH buffer is at least one of acetic acid, sodium acetate, disodium hydrogen phosphate, and sodium dihydrogen phosphate;
[0057] The dispersant is Avolan IS series from Tona Chemical;
[0058] The alkali agent is NaOH (mass concentration is 32.5%);
[0059] The reducing agent is hydrosulfur powder.
[0060] Preferably, the dyeing temperature is 130-135°C and the dyeing time is 40-45min;
[0061] Preferably, the total amount of environmentally friendly disperse dye red, environmentally friendly disperse dye yellow, and environmentally friendly disperse dye blue is 0.05%-0.3%;
[0062] Preferably, the amount of dispersant is 0.1%-0.3%;
[0063] Preferably, the pH buffer is used in an amount of 4%-7%;
[0064] Preferably, the reduction cleaning is performed at 75-85°C for 10-20 minutes;
[0065] Preferably, the amount of NaOH (mass concentration is 32.5%) is 0.3%-0.5%;
[0066] Preferably, the amount of hydrosulfite used is 0.2%-0.3%.
[0067] Beneficial Effects
[0068] The present invention belongs to the field of textile printing and dyeing technology in the printing and dyeing production of the textile industry, and in particular, relates to a bio-based oligomer remover and its preparation method and application. In the present invention, firstly, bio-based tall oil fatty acid is added to the reaction. The main source of raw materials for producing tall oil fatty acid is tall oil (Talloil), a byproduct produced by paper mills, also known as pulp floating oil, the main components of which are fatty acids and rosin acid, obtained from the surface of pine pulp and black liquor produced by the sulfate process, distilled and purified, and processed to produce tall oil fatty acid; secondly, bio-based twenty-one carbon dibasic acid is added to the reaction, which is a liquid dibasic acid prepared from vegetable oil fatty acids. Bio-based products can be completely biodegraded in the natural environment, are environmentally friendly and safe, and enhance the renewable and environmentally friendly value of the product; finally, natural oil sulfonated oil is added to the final product, which is an anionic sulfonated oil fatting agent made of natural oil as the main raw material, modified by sulfur trioxide gas sulfonation process, and then compounded with other necessary components, and is an excellent anionic surfactant. By utilizing the synergistic effect and synergistic effect of nonionic surfactants and anionic surfactants, the dispersion performance is improved, the "white powder" phenomenon of oligomers is improved, and a bio-based high-temperature oligomer remover with excellent performance is compounded to improve the dyeing leveling and dispersion effects of polyester fabrics, especially ultra-fine fibers, and improve product quality, which has significant social benefits and broad market prospects. DETAILED DESCRIPTION
[0069] The present invention is further described below in conjunction with examples, which are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0070] The materials and grades involved in the following examples and comparative examples are as follows:
[0071] (A) Bio-based organic fatty acids
[0072] A-1: Bio-based tall oil fatty acid, ALTAPYNE 1483
[0073] A-2: Bio-based hexanedicarboxylic acid, DIACID 1550
[0074] (B) Alcohol polymers
[0075] B-1: PEG600
[0076] (C) Oxidant
[0077] C-1: Hypophosphorous acid H3PO2
[0078] (D) Catalyst
[0079] D-1: Toluenesulfonic acid
[0080] (E) Natural oil sulfonated oil
[0081] E-1: RS sulfonated rapeseed oil
[0082] (F) Solvent
[0083] F-1: Diethylene glycol butyl ether
[0084] (G) Defoaming agent
[0085] G-1: Silicone defoamer CD-1100
[0086] G-2: Polyether defoamer CD-1116M
[0087] (H) Environmentally friendly disperse dyes
[0088] H-1: Red AC-E
[0089] H-2: Yellow AC-E
[0090] H-3: Blue AC-E
[0091] (I) pH buffer
[0092] I-1: pH 4.5 buffer
[0093] (J) Dispersant
[0094] J-1: Avolan IS
[0095] (K) Alkali
[0096] K-1: NaOH (mass concentration 32.5%)
[0097] (L) Reducing agent
[0098] L-1: Hydrosulfite
[0099] The preparation method of the bio-based oligomer remover comprises the following steps:
[0100] Step 1: Adding bio-based organic fatty acid into a reactor and stirring;
[0101] Step 2: Adding the alcohol polymer into the reactor and stirring;
[0102] Step 3, adding an oxidant into the reactor and stirring;
[0103] Step 4: Add the catalyst into the reactor and stir;
[0104] Step 5: Stir the materials evenly, and start heating to 150-155°C to melt;
[0105] Step 6: Continue to heat up to 235-240°C to carry out dehydration reaction;
[0106] Step 7, cooling to 180-190°C, and continuing the dehydration reaction;
[0107] Step 8: After the dehydration reaction is completed, the temperature is naturally lowered to below 45°C;
[0108] Step 9: Add 20%-30% natural oil sulfonated oil and stir
[0109] Step 10, adding 1%-5% solvent and stirring;
[0110] Step 11: Add 0.01%-1% defoamer and stir to obtain an oligomer remover.
[0111] Furthermore, in step 1, the stirring speed is 20-30 rpm, the temperature does not exceed 35° C., and nitrogen protection is introduced;
[0112] Furthermore, in step 5, stirring was maintained for 20 min, and nitrogen protection was introduced;
[0113] Furthermore, in step 6, the stirring speed is 55-65 rpm, the reaction time is 2 h, and nitrogen protection is introduced;
[0114] Furthermore, in step 7, after cooling to 180-190°C, the nitrogen is turned off, vacuum is drawn, and the reaction time is 20 minutes;
[0115] Furthermore, in step eight, first evacuate the chamber, introduce nitrogen, and then cool the chamber;
[0116] Further, in step nine, the stirring speed is 20-30 rpm, and the stirring is for 60 min;
[0117] Further, in step 10, the stirring speed is 20-30 rpm, and the stirring is performed for 10 min.
[0118] Furthermore, in step eleven, the stirring speed is 20-30 rpm, and the stirring is performed for 10 min.
[0119] Example 1 (raw materials and dosages used are shown in Table 1)
[0120] A bio-based oligomer remover is prepared from the following raw materials in the following mass ratios: 15% of ALTAPYNE 1483, 25% of DIACID 1550, 36% of PEG600, 0.2% of hypophosphorous acid H3PO2, 0.2% of toluenesulfonic acid, 25% of RS sulfonated rapeseed oil, 1.5% of diethylene glycol butyl ether, 0.02% of CD-1100, and 0.02% of CD-1116M;
[0121] The preparation method of the bio-based oligomer remover in this embodiment comprises the following steps:
[0122] (1) Add 150 g of ALTAPYNE 1483 and 250 g of DIACID 1550 into a reactor and stir at a speed of 20-30 rpm. The temperature should not exceed 35° C. and nitrogen should be introduced for protection.
[0123] (2) Add 360 g of PEG600 into the reactor and stir;
[0124] (3) Add 2 g of hypophosphorous acid H3PO2 into the reactor and stir;
[0125] (4) Add 2 g of toluenesulfonic acid into the reactor and stir;
[0126] (5) Stir the materials evenly and start heating to 150-155°C to melt them; keep stirring for 20 minutes and introduce nitrogen protection;
[0127] (6) Continue heating to 235-240°C for dehydration reaction; stirring speed is 55-65 rpm, reaction time is 2 h, and nitrogen protection is introduced;
[0128] (7) Cool down to 180-190°C, continue the dehydration reaction, turn off the nitrogen, evacuate, and the reaction time is 20 min;
[0129] (8) After the dehydration reaction is completed, the temperature is naturally lowered to below 45°C, vacuumed, and nitrogen is introduced;
[0130] (9) adding 250 g RS sulfonated rapeseed oil and stirring at a stirring speed of 20-30 rpm for 60 min;
[0131] (10) Add 15 g of diethylene glycol butyl ether and stir for 10 min;
[0132] (11) Add 0.2 g CD-1100 and 0.2 g CD-1116M, stir for 10 min, and filter the material.
[0133] Example 2 (raw materials and dosages used are shown in Table 1)
[0134] The preparation conditions and process in this embodiment are basically the same as those in Example 1, wherein the raw material ratio is as follows: ALTAPYNE1483 20%, DIACID 1550 20%, PEG600 36%, hypophosphorous acid H3PO2 0.1%, toluenesulfonic acid 0.1%, RS sulfonated rapeseed oil 25%, diethylene glycol butyl ether 1.5%, CD-1100 0.02%, CD-1116M 0.02%;
[0135] Example 3 (raw materials and dosages used are shown in Table 1)
[0136] The preparation conditions and process in this embodiment are basically the same as those in Example 1, wherein the raw material ratio is as follows: ALTAPYNE1483 15%, DIACID 1550 15%, PEG600 36%, hypophosphorous acid H3PO2 0.3%, toluenesulfonic acid 0.3%, RS sulfonated rapeseed oil 30%, diethylene glycol butyl ether 1.5%, CD-1100 0.02%, CD-1116M 0.02%;
[0137] Comparative Example 1
[0138] DISPERON G-55K is an oligomer remover, which is commonly used in the market and has a good overall effect. This is used as Comparative Example 1.
[0139] Table 1
[0140]
[0141]
[0142] Example 4 (raw materials and dosages used are shown in Table 2)
[0143] The dye liquor for disperse dye high-temperature immersion dyeing process prepared by using oligomer remover is made of the following raw materials in the following mass ratio: oligomer remover Example 1 0.2%, red AC-E 0.04%, yellow AC-E 0.04%, blue AC-E 0.04%, pH 4.5 buffer solution 5%, Avolan IS 0.2%; the raw material ratio of reducing cleaning liquid: oligomer remover Example 1 0.1%, NaOH (32.5%) 0.3%, and hydrosulfite 0.2%.
[0144] The preparation method and dyeing process of the dispersed high temperature immersion dyeing process in this embodiment include the following steps:
[0145] (1) Weigh 0.4 g each of red AC-E, yellow AC-E, and blue AC-E, dissolve them in 100 ml of water to prepare a 4 g / l dye solution for later use;
[0146] (2) Add 0.4 g of oligomer remover Example 1, 0.4 g of Avolan IS, 10 g of pH 4.5 buffer and 29.2 g of water to a 300 ml dye cup and stir well with a glass rod;
[0147] (3) Use a 20 ml fat-belly pipette to transfer 20 ml of each of 4 g / l red AC-E, yellow AC-E, and blue AC-E into a 300 ml dye cup. The total amount of solution in the dye cup is 200 g.
[0148] (4) High temperature dyeing bath ratio 1:20, total dyeing liquid 200g, dyeing polyester fabric 10g. Put 10g polyester fabric into a 300ml dyeing cup and tighten the lid of the dyeing cup;
[0149] (5) Place the dye cup in an infrared high-temperature dyeing machine, heat the dyeing machine to 130-135°C, heat up at a rate of 1°C / 1min, keep warm for 45min, and cool to below 45°C after the heat preservation.
[0150] (6) Take out the polyester colored cloth from the dye cup and rinse it with clean water;
[0151] (7) preparing a reducing cleaning solution by weighing 0.2 g of the oligomer remover example, 0.6 g of NaOH (32.5%), 0.4 g of hydrosulfite and 198.8 g of water at a temperature of 80° C., and soaking the polyester colored cloth in the reducing cleaning solution for 20 min;
[0152] (8) Take out, rinse with clean water, dehydrate, and dry in an oven at 80°C.
[0153] Example 5 (raw materials and dosages used are shown in Table 2)
[0154] The preparation conditions and process in this embodiment are basically the same as those in Embodiment 4. The raw material ratios of the dye solution are as follows: oligomer remover embodiment 2 0.2%, red AC-E 0.04%, yellow AC-E 0.04%, blue AC-E 0.04%, pH 4.5 buffer 5%, Avolan IS 0.2%; the raw material ratios of the reducing cleaning solution are: oligomer remover embodiment 1 0.1%, NaOH (32.5%) 0.3%, and hydrosulfite 0.2%.
[0155] Example 6 (raw materials and dosages used are shown in Table 2)
[0156] The preparation conditions and process in this embodiment are basically the same as those in Embodiment 4. The raw material ratios of the dye solution are as follows: oligomer remover embodiment 3 0.2%, red AC-E 0.04%, yellow AC-E 0.04%, blue AC-E 0.04%, pH 4.5 buffer 5%, Avolan IS 0.2%; the raw material ratios of the reducing cleaning solution are: oligomer remover embodiment 1 0.1%, NaOH (32.5%) 0.3%, and hydrosulfite 0.2%.
[0157] Comparative Example 2 (raw materials and dosages used are shown in Table 2)
[0158] The preparation conditions and process of this embodiment are basically the same as those of Embodiment 4, wherein the raw material ratio of the dye solution is as follows: oligomer remover comparative example 1 0.2%, red AC-E 0.04%, yellow AC-E 0.04%, blue AC-E 0.04%, pH 4.5 buffer 5%, Avolan IS 0.2%; the raw material ratio of the reducing cleaning solution is: oligomer remover embodiment 1 0.1%, NaOH (32.5%) 0.3%, and hydrosulfite 0.2%.
[0159] Table 2
[0160]
[0161] Excellent as a high temperature and high pressure dispersed oligomer remover for polyester fibers, it must be suitable for rapid dyeing process. It can maintain dyeing under acidic conditions, effectively avoiding the color deviation of the cloth caused by hydrolysis of sensitive dyes. It does not contain carrier components, which helps to improve the working environment. It is suitable for high temperature dark dyeing of polyester and high temperature light dyeing that requires warm tones. Therefore, the specific requirements for oligomer removers can be reflected by the following performances:
[0162] 1. Storage stability
[0163] Place 100g of sample in an oven at 50℃ for 24h, and observe the appearance of the solution: whether the solution is stratified, whether there is condensation or oil floating out. The test results are shown in Table 3.
[0164] 2. Dispersibility
[0165] Weigh 0.4g of dispersed dark blue HGL 200%, 0.1g of oligomer remover, 5g of pH 4.5 buffer and 94.5g of water to make 100ml of dye solution and stir for 10min; put a piece of Qualitative filter paper is placed on the filter paper and pressed with a stainless steel ring. The vacuum pump is turned on and the pressure is set to the maximum. 100 ml of dye solution is poured into the Buchner funnel, the filtration time is recorded, and the dye residue on the filter paper is observed. The higher the rating, the better. The test results are shown in Table 3.
[0166] Room temperature dispersibility: prepare 100 ml of dye solution at room temperature and filter at room temperature;
[0167] High temperature dispersibility: Heat the prepared 100 ml dye solution to 130℃ in an infrared dyeing machine, keep it warm for 30 minutes, then reduce it to 80℃, take it out and filter it (the Buchner funnel must be soaked in 80℃ water);
[0168] Residue rating scale: 5 none, 4 a little, 3 some, 2 a lot, 1 very heavy
[0169] 3. Transferability
[0170] Weigh 0.1g high temperature dispersed oligomer remover and 100g water to prepare 100ml oligomer remover solution; sew the same size colored cloth and white cloth around, the total weight of the cloth is 5g; put the experimental cloth and 100ml aqueous solution into a 200ml dye cup as a blank sample; put the experimental cloth and 100ml oligomer remover solution into a 200ml dye cup as a test sample; put the dye cup into an infrared dyeing machine and heat it to 130℃, keep it warm for 30 minutes, cool it to room temperature, take out the test experimental cloth, wash it with water, and dry it. Observe the intensity and color change of the color-shifted cloth with oligomer remover added and the blank original color-shifted cloth, and the coloring performance of the white cloth. The higher the rating, the better. The test results are shown in Table 3.
[0171] Rating standard: 5. The strength of the oligomer remover color-shifted cloth is more than 10% lower than the blank color-shifted cloth, and there is no obvious color jump phenomenon;
[0172] 3. The strength of the oligomer remover-displaced cloth and the blank-displaced cloth varies within 5%, and there is no obvious color jump phenomenon;
[0173] 1. The strength of the oligomer remover discolored cloth is within 10% of the strength of the blank discolored cloth or there is obvious color jump phenomenon;
[0174] Table 3
[0175]
[0176] 4. Slow-dyeing
[0177] According to the component ratio in Table 2, add oligomer remover to prepare 200ml polyester immersion dye solution, and do not add any oligomer remover to the blank dye solution. Pour into 300ml dye cups respectively, add 2g polyester standard white cloth, heat the dye cup from 30℃ to 130℃ in the infrared dyeing machine, keep warm for 45 minutes, and cool down to below 45℃. During the heating process, keep warm at 90℃, 100℃, 110℃, 120℃, 130℃, and 130℃ for 30 minutes respectively, take out the colored cloth, and add new 2g white cloth to the same residual night dye cup to continue dyeing. When the dyeing process is all over, take out the residual night dyed cloth sample, wash it with water, and dry it. Observe the dyeing rate comparison of the sample cloth with oligomer remover, the residual night dyed cloth sample and the blank dye solution. The higher the rating, the better. The test results are shown in Table 4.
[0178] Rating standard: 5. The dyeing speed of dyed sample cloth and residual night dyed sample cloth is slower than that of blank cloth, and there is no obvious color jumping phenomenon;
[0179] 3. The dyeing speed of the dyed sample and the residual night dyed sample is close to that of the blank, and there is no obvious color jumping phenomenon;
[0180] 1. The dyeing speed of the dyed sample and the leftover dyed sample is faster than that of the blank or there is obvious color jumping phenomenon;
[0181] Table 4
[0182] sample Example 4 Example 5 Example 6 Comparative Example 2 Slow-dyeing 3-5 3 3-5 3
[0183] 5. Determination of oligomer content on fabric by chloroform extraction method
[0184] Based on the principle of like dissolves like, an organic solvent is selected to dissolve the oligomer. Chloroform is selected as the extractant because it is small in size and can easily penetrate into the fiber.
[0185] Take 4g of dyed polyester fabric sample, cut into pieces less than 25mm2, weigh 3 samples of 1.0g (accurate to 0.01g) from the pieces, and place them in conical flasks. Add 50mL of chloroform respectively, seal the conical flask with a film, place it in a water bath at 80℃, and keep vigorous shaking for 2h. After shaking, place the sample on a rotary evaporator for evaporation (wash the conical flask with chloroform 3 times, and pour the washing liquid into the evaporating flask). When the volume of the liquid in the evaporating flask is 5mL, place it under a nitrogen blow dryer to dry it. The evaporating flask is weighed on an electronic balance before adding the liquid, and the liquid is poured in and weighed on an electronic balance after evaporation. The difference between the two masses is the mass of the oligomer. The test results are shown in Table 5. The lowest value indicates the lowest oligomer content.
[0186] Table 5 Residual oligomer content on fabric (mg)
[0187] sample Example 4 Example 5 Example 6 Comparative Example 2 1# 15.2 14.3 13.6 14.5 2# 14.5 14.9 13.8 15.1 3# 14.1 13.7 13.1 13.9
[0188] It can be seen from the results of Table 3, Table 4 and Table 5 that the basic performance of the bio-based oligomer remover prepared by the present invention is better than that of Comparative Example 1 or similar to that of Comparative Example 1; from the comparison between Example 3 and Comparative Example 1, it can be seen that the natural fat sulfonated oil is adsorbed on the surface of the dye particles to form a strong negative charge layer, so that there is a strong electric repulsion between the dye particles to form a stable dispersed state, and has a strong dispersing ability for the aggregates of disperse dyes, thereby reducing its cohesion, so that the dye remains stable in the dye solution at 130°C, the slow dyeing effect is obvious, and the dispersion performance of the dye and polyester oligomer under high temperature is significantly improved; from the comparison between Example 1, Example 2 and Example 3, it can be seen that the amount of bio-based organic fatty acid can improve the migration performance of the dye; the synergistic effect and synergistic effect of non-ionic surfactants and anionic surfactants are used to compound a bio-based oligomer remover with excellent performance, improve the leveling effect of fabrics, especially the leveling and dispersion effect of ultrafine fibers, improve product quality, and have significant social benefits and broad market prospects.
[0189] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the bio-based oligomer remover, preparation method and application of the present invention, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A bio-based oligomer remover, characterized in that: Made of the following raw materials in the following mass ratios: bio-based tall oil fatty acid ALTAPYNE 1483 15%, bio-based hexanedicarboxylic acid DIACID 1550 25%, PEG600 36%, hypophosphorous acid H3PO2 0.2%, toluenesulfonic acid 0.2%, RS sulfonated rapeseed oil 25%, diethylene glycol butyl ether 1.5%, silicone defoamer CD-1100 0.02%, polyether defoamer CD-1116M 0.02%; The preparation method of the bio-based oligomer remover comprises the following steps: (1) Add 150 g of bio-based tall oil fatty acid ALTAPYNE 1483 and 250 g of bio-based heneicosadicarboxylic acid DIACID1550 into a reactor and stir at a stirring speed of 20-30 rpm, a temperature not exceeding 35°C, and nitrogen protection; (2) Add 360 g of PEG600 into the reactor and stir; (3) Add 2 g of hypophosphorous acid H3PO2 into the reactor and stir; (4) Add 2 g of toluenesulfonic acid into the reactor and stir; (5) Stir the materials evenly and start heating to 150-155°C to melt them; keep stirring for 20 minutes and introduce nitrogen protection; (6) Continue to raise the temperature to 235-240°C for dehydration reaction; stir at 55-65 rpm, reaction time 2 h, and introduce nitrogen protection; (7) Cool down to 180-190°C, continue the dehydration reaction, turn off the nitrogen, evacuate, and the reaction time is 20 min; (8) After the dehydration reaction is completed, the temperature is naturally lowered to below 45°C, vacuum is drawn, and nitrogen is introduced; (9) Add 250 g RS sulfonated rapeseed oil and stir at a speed of 20-30 rpm for 60 min; (10) Add 15 g of diethylene glycol butyl ether and stir for 10 min; (11) Add 0.2 g of silicone defoamer CD-1100 and 0.2 g of polyether defoamer CD-1116M, stir for 10 min, and filter the material.
Citation Information
Patent Citations
Method for synthesizing polyethyleneglycol ditall oleate
CN101633732A
Oligomer removing agent for polyester-based fiber material
CN102433779A
Oligomer removing agent and preparation method thereof
CN104558566A
Method for dyeing polyester fiber type material by using oligomer removing agent
CN104562776A
Low-polymer protective agent and preparation method thereof
CN106351040A