An organic matter degradation catalyst with heavy metal adsorption function and its preparation method and application
By preparing catalysts with core-shell structures such as red mud, steel slag and titanium-containing slag, the problem of difficult-to-degrade organic matter and heavy metal pollution in existing water treatment technologies is solved, and the rapid and efficient degradation of complex polluted wastewater is achieved. and heavy metal adsorption reduces cost and complexity.
Patent Information
- Application Number
- CN202211729008.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-30
AI Technical Summary
When existing water treatment technologies deal with difficult-to-degrade organic matter and heavy metal pollution, there are problems such as photocatalytic dependence, complex ozone oxidation system, high raw material cost and complex preparation process. In addition, the utilization rate of industrial solid waste is low, making it difficult to effectively treat complex polluted wastewater.
The catalyst with heavy metal adsorption function is used to form a core-shell structure by decaling, granulating and sintering solid waste such as red mud, steel slag and titanium-containing slag to form a catalyst with core-shell structure, which has photocatalytic oxidation and Fenton oxidation. It can effectively adsorb and degrade heavy metals and organic pollutants in wastewater.
It realizes rapid and efficient degradation of heavy metals and organic pollutants in complex polluted wastewater, reduces raw material costs, simplifies the preparation process, improves solid waste utilization, and is suitable for the treatment of complex polluted wastewater.
Smart Images

Figure CN115945200B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a water treatment material, in particular to an organic matter degradation catalyst with heavy metal adsorption function, and also to a preparation method and application of the catalyst in wastewater treatment, belonging to the technical field of wastewater treatment. Background Art
[0002] At present, the research on the construction of catalytic systems for refractory organic matter in water mainly focuses on photocatalytic technology and ozone oxidation technology. However, photocatalytic water treatment is easily affected by water quality, weather and other conditions, and ozone-based technology requires complex ozone generation and exhaust gas discharge systems, which is not conducive to the further development and application of catalytic loading materials. Compared with photocatalytic technology and ozone oxidation technology, advanced oxidation technology does not require the stimulation of light sources or the existence of complex gas systems. It can effectively remove organic pollutants under the conditions of the presence of catalysts and oxidants, but it also has problems such as high raw material costs and complex preparation processes.
[0003] At the same time, textile wastewater, electroplating wastewater, metallurgical wastewater, etc. will produce wastewater rich in metal ions such as copper, lead, and chromium during the working process. If these metal ions are properly treated, they can be used to a very high degree. If they are not treated well, these metal ions will be in the wastewater, which will cause considerable pollution to the environment. Therefore, it is imperative to treat heavy metal industrial wastewater.
[0004] The stockpile of industrial solid waste is huge. Solid waste resources such as titanium-containing blast furnace slag, Bayer red mud, and steel slag are rich in valuable metal elements, but they are difficult to extract and have low utilization rates. If they are used to prepare solid waste-based catalysts and heavy metal adsorbents, it will not only achieve high-value utilization of solid waste, but also promote the rapid development of traditional water treatment catalysts. Summary of the invention
[0005] In view of the defects of the prior art, the purpose of the present invention is to provide an organic matter degradation catalyst with heavy metal adsorption function, which can not only adsorb heavy metal ions such as chromium, lead, cadmium, copper, etc. in water bodies, but also has photocatalytic oxidation and Fenton oxidation catalytic effects, and can achieve rapid and efficient degradation of phenol, bisphenol A, organic dyes, etc. in wastewater, and is particularly suitable for the treatment of complex polluted wastewater.
[0006] The second object of the present invention is to provide a method for preparing an organic matter degradation catalyst with heavy metal adsorption function. The preparation method uses solid wastes such as titanium-containing slag, red mud, and steel slag as raw materials. The raw material cost is low and the added value is high. It can achieve waste treatment with waste, with significant social and ecological benefits. The preparation process is simple and the industrialization requirements are low.
[0007] The third object of the present invention is to provide an application of an organic matter degradation catalyst with heavy metal adsorption function. When added to wastewater, it can not only efficiently adsorb heavy metal ions such as chromium, lead, cadmium, and copper in the water, but also has photocatalytic oxidation and Fenton oxidation catalytic effects, and can achieve rapid and efficient degradation of phenol, bisphenol A, organic dyes, etc. in the wastewater, and is particularly suitable for the treatment of complex polluted wastewater.
[0008] In order to achieve the above technical objectives, the present invention provides a method for preparing an organic matter degradation catalyst with heavy metal adsorption function, the method comprising dealkalizing, granulating I and sintering I red mud to obtain red mud solidified particles, and granulating II and sintering II the red mud solidified particles and raw materials including steel slag and titanium-containing slag to obtain.
[0009] The schematic diagram of the catalyst structure prepared by the technical solution of the present invention is as follows Figure 1 As shown in the scanning electron microscope image Figure 2 As shown: The catalyst has a "core-shell structure", with its core being solidified red mud particles, and its shell being formed by the accumulation of steel slag particles and titanium-containing slag particles, and a large number of pores are retained between the particles. The core of the solidified red mud particles is formed by the agglomeration of many extremely fine primary particles, which have the characteristics of high surface area, strong alkalinity, and high activity. After the primary particles are dealkalized and calcined, the specific surface area is further improved, and the adsorption effect of heavy metals is enhanced. At the same time, the calcination modification activates its mineral composition, making it have a certain reactivity. Some heavy metals such as manganese, cobalt, chromium, copper, zinc and other metal ions will react with active minerals to produce precipitation, realizing the chemical removal of heavy metal ions. The steel slag particles and titanium-containing slag particles adhere to the surface of the red mud solidified particles. Both contain a large amount of catalytically active metal components, such as manganese, iron, titanium, etc., which give the composite catalyst excellent catalytic activity. For example, titanium dioxide has photocatalytic oxidation activity, while iron oxides and iron oxides have advanced oxidation catalytic activity. At the same time, the steel slag particles and titanium-containing slag particles are accumulated into a porous, irregular shell structure, which can also improve the catalyst's adsorption performance for heavy metals.
[0010] As a preferred solution, the process of dealkalization is: red mud is mixed with lime and water in a mass ratio of 1: (0.05-0.2): (1-3) for reaction. Red mud is preferably Bayer red mud. The reaction time is 30-50 minutes. Red mud is mixed with lime and water for reaction, and the heat released by lime is used to heat the reaction to complete the dealkalization and modification of red mud. Based on the adsorption process of heavy metals in water, there is also an electrostatic adsorption effect. When the pH value of the water body is greater than the pH value of red mud, the surface of red mud particles will be negatively charged, which will form electrostatic attraction with positively charged heavy metal ions, thereby achieving the purpose of removing heavy metals. The alkali content in red mud is too high, so dealkalization treatment is carried out on it, which is beneficial to improve the adsorption performance of catalytic materials for heavy metal ions.
[0011] As a preferred solution, the granulation I is granulated by spraying, and the particle size of the granules is controlled to be 10-15 microns. Spray drying allows the red mud slurry to solidify and form quickly, and granules with relatively uniform particle size distribution can be obtained.
[0012] As a preferred solution, the conditions of sintering I are: sintering at a temperature of 800-900° C. for 1-2.5 hours. The sintering process mainly solidifies the particles, and the red mud can be activated and modified during the sintering process. Under the preferred sintering conditions, all the adsorbed water and crystallized water in the red mud will be discharged, and most of the calcite and hydrous minerals will be decomposed, and part of the hematite will begin to transform, so that its ability to adsorb heavy metal ions and its reaction activity with heavy metal ions are improved.
[0013] As a preferred solution, the titanium content of the titanium-containing slag is greater than 15%, preferably greater than 24%. The titanium-containing slag is for example titanium-containing blast furnace slag.
[0014] As a preferred solution, the total mass ratio of red mud solidified particles to titanium-containing slag and steel slag is 15-30:60-100; wherein, the mass ratio of titanium-containing slag to steel slag is 40-60:20-40. If the mass ratio of red mud solidified particles is too low, the adsorption performance of the catalyst for heavy metal ions will be reduced, while if the mass ratio of red mud solidified particles is too high, it will be difficult for titanium-containing slag and steel slag to form a complete shell on the surface of red mud solidified particles. If the ratio of titanium-containing slag to steel slag is too low, its photocatalytic activity will be reduced, while if the ratio of titanium-containing slag to steel slag is too high, its Fenton oxidation catalytic activity will be affected.
[0015] As a preferred solution, the raw material comprises silica sol, and the mass of the silica sol is 2-15% of the mass of the solidified red mud particles. The silica sol is used as a binder.
[0016] As a preferred solution, the granulation II adopts a three-dimensional mixing granulation method. The three-dimensional mixing granulation method is mainly used to make the titanium-containing slag powder and the steel slag powder evenly adhere to the surface of the solidified red mud particles.
[0017] As a preferred solution, the sintering conditions of the sintering II are: sintering at 550-650°C for 1-3h. If the temperature is too low, the catalyst has a low consolidation strength, the structure is easy to change during use, and the stability is poor; if the temperature is too high, the useful components such as titanium dioxide will undergo a crystal transformation and lose catalytic activity.
[0018] The invention also provides an organic matter degradation catalyst with heavy metal adsorption function, which is obtained by the preparation method.
[0019] The present invention also provides an organic matter degradation catalyst with heavy metal adsorption function, which is applied to heavy metal adsorption and / or catalytic degradation of organic matter in water bodies.
[0020] As a preferred solution, the catalyst is used in the process of catalyzing the degradation of organic matter, and auxiliary agents including hydrogen peroxide, citric acid and ozone are added, wherein hydrogen peroxide and citric acid are mixed and added before use, and ozone is added separately during the application process.
[0021] The method for preparing the organic matter degradation catalyst with heavy metal adsorption function of the present invention comprises the following steps:
[0022] 1) weighing and mixing red mud, lime and water in a ratio of 1:(0.05-0.2):(1-3) to carry out dealkalization reaction for 30-50 minutes;
[0023] 2) Filter the slurry red mud after dealkalization treatment to remove large particles to meet the spraying requirements, continue to add water according to the ratio of slurry: water = 1: 1.5-2.5, use a spray drying tower for granulation, and obtain red mud particles with a particle size of 10-15 microns;
[0024] 3) Sinter and solidify the red mud particles at 800-900°C for 1-2.5 hours and set aside.
[0025] 4) The steel slag needs to be screened to remove the larger iron-rich particles.
[0026] 5) Weigh titanium-containing slag and steel slag in proportion, and use a jet mill to grind them fully to a particle size of 1 to 3 μm;
[0027] 6) Red mud particles and silica sol are weighed at a ratio of 1: (0.02-0.1) and mixed in a three-dimensional mixer for 30-40 minutes; then titanium-containing blast furnace slag and steel slag powder are mixed in a three-dimensional mixer for 15-20 minutes to wrap the red mud particles to form agglomerates (such as Figure 1 The agglomerate particles are sintered at 550-650°C for 1-3 hours to solidify, thereby obtaining a catalyst.
[0028] The invention discloses an application of an organic matter degradation catalyst with heavy metal adsorption function. The catalyst is used in combination with auxiliary additives including hydrogen peroxide, citric acid and ozone to degrade organic matter such as phenol, bisphenol A and organic dyes in wastewater. The catalyst itself has good adsorption performance and can adsorb heavy metal ions in wastewater. The wastewater environment temperature of the catalyst is 20-30 DEG C. The catalytic time is generally 30-50 minutes according to the concentration. The removal rate of organic pollutants such as phenol within the reaction time is more than 97%, and the heavy metal adsorption can reach more than 80%. The amount of the catalyst added to the wastewater is 20-40 g / L. The hydrogen peroxide (added in the form of hydrogen peroxide) and citric acid are prepared into a mixed liquid according to the ratio of =1:(1.7-2.3). The added concentration of the mixed liquid in the wastewater is 3.5-5.5 g / L. At the same time, after the water treatment filtration process starts, an ozone solution is added at 1.5-1.9 g / L.
[0029] The catalyst of the invention is particularly suitable for treating printing and dyeing wastewater. The main pollutants in the printing and dyeing wastewater are: difficult-to-degrade complex organic substances mainly including inorganic oil, lanolin, biodegradable surfactant, polyvinyl alcohol slurry, and starch ether; difficult-to-degrade organic substances mainly including polymer impurities, slurry, synthetic polymer finishing agent, and silicone; and toxic pollutants mainly including formaldehyde, organic metals, cationic retarder, complex, and heavy metal salts (chromium, copper, mercury, cadmium, and antimony). According to different products and processes, the COD concentration in the wastewater is generally 400-1000 mg / L, copper is 0.5-1 mg / L, cadmium is 0.01-0.1 mg / L, and antimony is 0.01-0.05 mg / L. According to the national quality standard for surface water, all of them exceed the minimum five-category water standard.
[0030] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0031] The core of the organic matter degradation catalyst with heavy metal adsorption function of the present invention is a porous spherical particle with certain mechanical strength obtained by red mud through dealkalization modification, spray drying and sintering solidification, which gives the catalytic material good heavy metal adsorption performance and good chemical reaction activity, and can adsorb or react to passivate heavy metal elements such as chromium, cadmium, lead, copper, zinc, arsenic, etc. in water. The outside of the red mud particles is adhered to titanium-containing slag and steel slag, which contain a large amount of transition metals such as manganese and vanadium, as well as titanium dioxide with photoelectric effect. The titanium content in the titanium-containing slag is high, and titanium dioxide is mainly present. After being irradiated with ultraviolet light, photogenerated electrons are generated, holes are generated in the valence band, and the holes oxidize and adsorb organic matter on the surface of the particles, or activate hydroxide in water into hydroxyl radicals, thereby realizing photocatalytic oxidation. Red mud, steel slag and titanium-containing slag all contain a large amount of transition metal elements such as manganese and vanadium, and transition metal elements can generate active oxygen molecules by activating hydrogen peroxide or persulfate to attack organic matter, causing it to break the chain and realize catalytic degradation. Based on this, the catalyst of the present invention has both photocatalytic and metal catalytic functions, and can also realize the adsorption of heavy metals.
[0032] The preparation method of the organic matter degradation catalyst with heavy metal adsorption function of the present invention uses solid wastes such as titanium-containing slag, red mud, steel slag, etc. as raw materials, has low cost and high added value, can achieve waste treatment with waste, has significant social and ecological benefits, and has a simple preparation process and low industrialization requirements.
[0033] The organic matter degradation catalyst with heavy metal adsorption function of the present invention is added to wastewater at a low concentration. In a short reaction time, the removal rate of organic pollutants such as phenol is more than 97%, and the heavy metal adsorption can reach more than 80%. It can be widely used in the treatment process of complex wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a schematic diagram of the structure of the catalyst particles prepared in Example 1.
[0035] Figure 2 This is an electron microscope photograph of the catalyst particles prepared in Example 1. DETAILED DESCRIPTION
[0036] The following examples are intended to further illustrate the present invention in detail, but are not intended to limit the scope of protection of the claims of the present invention.
[0037] Unless otherwise specified in the following examples and comparative examples, the chemical reagents used are all conventional chemical reagents.
[0038] The COD of the printing and dyeing wastewater used in each embodiment and comparative embodiment is 600 mg / L and various heavy metals exceed the fifth category water standard for surface water.
[0039] Example 1
[0040] Step 1: sieve the Bayer red mud to remove particles with a particle size greater than 200 μm, then weigh 1000 parts of red mud, 150 parts of lime, and 2000 parts of water at a rate of 10 g per part, react for 35 minutes, and then pass the slurry through a 200-mesh sieve;
[0041] Step 2: The slurry after sieving is prepared into a slurry suitable for spray granulation with a ratio of slurry: water = 1:2. 100 parts of slurry and 200 parts of water are weighed. After spray granulation, the powder with a particle size of 15 microns is selected and reserved for use;
[0042] Step 3: The powder obtained in step 2 is pre-calcined at 850° C. for 1.5 h in a muffle furnace to further solidify the granulated powder, and then removed for later use after natural cooling;
[0043] Step 4: 400 parts of 17% titanium-containing blast furnace slag and 300 parts of steel slag are weighed in proportion, and ground into particles with a particle size of 1 μm using a jet mill.
[0044] Step 5: Weigh 20 parts of red mud solidified particles at 10 g each, weigh 3 parts of silica sol, place them in a three-dimensional mixer and mix for 15 minutes, continue to weigh 60 parts of titanium-containing blast furnace slag and steel slag powder, mix the powders, place them in the mixer, and mix for 20 minutes to obtain agglomerate particles.
[0045] Step 6: The obtained agglomerate particles are sintered at 650° C. for 2 h to solidify to obtain a catalyst.
[0046] Step 7: Weigh 10 parts of hydrogen peroxide solution (30%) and 20 parts of citric acid, stir for 3 minutes, and obtain an auxiliary agent.
[0047] Step 7: Add 60g of catalyst to 2kg of printing and dyeing wastewater, add 9g of auxiliary agent and 3.6g of ozone, maintain the water temperature at 25°C, and measure the COD and heavy metal content in the water after 30 minutes of reaction.
[0048] Example 2
[0049] Step 1: sieve the Bayer red mud to remove particles with a particle size greater than 200 μm, then weigh 1000 parts of red mud, 100 parts of lime, and 1800 parts of water at a weight of 10 g per part, react for 35 minutes, and then pass the slurry through a 200-mesh sieve;
[0050] Step 2: The slurry after sieving is prepared into a slurry suitable for spray granulation with a ratio of slurry: water = 1:2. 100 parts of slurry and 200 parts of water are weighed. After spray granulation, the powder with a particle size of 15 microns is selected and reserved for use;
[0051] Step 3: pre-calculate the powder obtained in step 2 at 900° C. for 1 hour using a muffle furnace to further solidify the granulated powder, and remove it for later use after natural cooling;
[0052] Step 4: 600 parts of 15% titanium-containing blast furnace slag and 200 parts of steel slag are weighed in proportion, and ground into particles with a particle size of 1 μm using a jet mill.
[0053] Step 5: Weigh 30 parts of red mud solidified particles at 10 g per part, weigh 2.5 parts of silica sol, place them in a three-dimensional mixer and mix for 20 minutes, then weigh 80 parts of titanium-containing blast furnace slag and steel slag powder, mix the powders in the mixer, mix for 20 minutes, and obtain agglomerate particles.
[0054] Step 6: The obtained agglomerate particles are sintered at 600° C. for 2 h to solidify to obtain a catalyst.
[0055] Step 7: Weigh 10 parts of hydrogen peroxide solution (30%) and 20 parts of citric acid, stir for 3 minutes, and obtain an auxiliary agent.
[0056] Step 7: Add 40g of catalyst to 2kg of printing and dyeing wastewater, add 7g of auxiliary agent and 3g of ozone at the same time, maintain the water temperature at 25°C, and measure the COD and heavy metal content in the water after 40 minutes of reaction.
[0057] Example 3
[0058] Step 1: sieve the Bayer red mud to remove particles with a particle size greater than 200 μm, then weigh 1000 parts of red mud, 200 parts of lime, and 2000 parts of water at a weight of 10 g per part, react for 35 minutes, and then pass the slurry through a 200-mesh sieve;
[0059] Step 2: The slurry after sieving is prepared into a slurry suitable for spray granulation with a ratio of slurry: water = 1:2. 100 parts of slurry and 200 parts of water are weighed. After spray granulation, the powder with a particle size of 15 microns is selected and reserved for use;
[0060] Step 3: pre-calcine the powder obtained in step 2 at 800° C. for 2.5 h in a muffle furnace to further solidify the granulated powder, and remove it for later use after natural cooling;
[0061] Step 4: 400 parts of 17% titanium-containing blast furnace slag and 400 parts of steel slag are weighed in proportion, and ground into particles with a particle size of 1 μm using a jet mill.
[0062] Step 5: Weigh 30 parts of red mud solidified particles at 10 g each, weigh 3 parts of silica sol and place them in a three-dimensional mixer for mixing for 30 minutes, then weigh 100 parts of titanium-containing blast furnace slag and steel slag powder, mix the powders and place them in the mixer for 20 minutes to obtain agglomerate particles.
[0063] Step 6: The obtained agglomerate particles are sintered at 650° C. for 2 h to solidify to obtain a catalyst.
[0064] Step 7: Weigh 10 parts of hydrogen peroxide solution (30%) and 17 parts of citric acid, stir for 3 minutes, and obtain an auxiliary agent.
[0065] Step 7: Add 80g of catalyst to 2kg of printing and dyeing wastewater, add 10g of auxiliary agent and 3.8g of ozone at the same time, maintain the water temperature at 25°C, and measure the COD and heavy metal content in the water after 35 minutes of reaction.
[0066] Comparative Example 1
[0067] Step 1: sieve the Bayer red mud to remove particles with a particle size greater than 200 μm, then weigh 1000 parts of red mud, 150 parts of lime, and 2000 parts of water at a weight of 10 g per part, perform hydrothermal reaction for 35 minutes, and then pass the slurry through a 200-mesh sieve;
[0068] Step 2: The slurry after sieving is prepared into a slurry suitable for spray granulation with a ratio of slurry: water = 1:2. 100 parts of slurry and 200 parts of water are weighed. After spray granulation, the powder with a particle size of 15 microns is selected and reserved for use;
[0069] Step 3: The powder obtained in step 2 is pre-calcined at 1050° C. for 1.5 h in a muffle furnace to further solidify the granulated powder, and then removed for standby after natural cooling;
[0070] Step 4: 400 parts of 17% titanium-containing blast furnace slag and 300 parts of steel slag are weighed in proportion, and ground into particles with a particle size of 1 μm using a jet mill.
[0071] Step 5: Weigh 10 parts of red mud solidified particles at 10 g each, weigh 3 parts of silica sol, place them in a three-dimensional mixer and mix for 15 minutes, then weigh 60 parts of titanium-containing blast furnace slag and steel slag powder, mix the powders, place them in the mixer, and mix for 20 minutes to obtain agglomerate particles.
[0072] Step 6: The obtained agglomerate particles are sintered at 650° C. for 2 h to solidify to obtain a catalyst.
[0073] Step 7: Weigh 10 parts of hydrogen peroxide solution (30%) and 20 parts of citric acid, stir for 3 minutes, and obtain an auxiliary agent.
[0074] Step 7: Add 60g of catalyst to 2kg of printing and dyeing wastewater, add 9g of auxiliary agent and 3.6g of ozone, maintain the water temperature at 25°C, and measure the COD and heavy metal content in the water after 30 minutes of reaction.
[0075] Comparative Example 2
[0076] Step 1: sieve the Bayer red mud to remove particles with a particle size greater than 200 μm, then weigh 1000 parts of red mud, 100 parts of lime, and 1800 parts of water at a weight of 10 g per part, perform hydrothermal reaction for 35 minutes, and then pass the slurry through a 200-mesh sieve;
[0077] Step 2: The slurry after sieving is prepared into a slurry suitable for spray granulation with a ratio of slurry: water = 1:2. 100 parts of slurry and 200 parts of water are weighed. After spray granulation, the powder with a particle size of 15 microns is selected and reserved for use;
[0078] Step 3: pre-calculate the powder obtained in step 2 at 900° C. for 1 hour using a muffle furnace to further solidify the granulated powder, and remove it for later use after natural cooling;
[0079] Step 4: 320 parts of 10% titanium-containing blast furnace slag and 180 parts of steel slag are weighed in proportion, and ground into particles with a particle size of 1 μm using a jet mill.
[0080] Step 5: Weigh 30 parts of red mud solidified particles at 10 g per part, weigh 2.5 parts of silica sol, place them in a three-dimensional mixer and mix for 20 minutes, then weigh 80 parts of titanium-containing blast furnace slag and steel slag powder, mix the powders in the mixer, mix for 20 minutes, and obtain agglomerate particles.
[0081] Step 6: The obtained agglomerate particles are sintered at 600° C. for 2 h to solidify to obtain a catalyst.
[0082] Step 7: Weigh 10 parts of hydrogen peroxide solution (30%) and 20 parts of citric acid, stir for 3 minutes, and obtain an auxiliary agent.
[0083] Step 7: Add 40g of catalyst to 2kg of printing and dyeing wastewater, add 7g of auxiliary agent and 3g of ozone at the same time, maintain the water temperature at 25°C, and measure the COD and heavy metal content in the water after 40 minutes of reaction.
[0084] Comparative Example 3
[0085] Step 1: sieve the Bayer red mud to remove particles with a particle size greater than 200 μm, then weigh 1000 parts of red mud, 200 parts of lime, and 2000 parts of water at a weight of 10 g per part, perform hydrothermal reaction for 35 minutes, and then pass the slurry through a 200-mesh sieve;
[0086] Step 2: The slurry after sieving is prepared into a slurry suitable for spray granulation with a ratio of slurry: water = 1:2. 100 parts of slurry and 200 parts of water are weighed. After spray granulation, the powder with a particle size of 15 microns is selected and reserved for use;
[0087] Step 3: pre-calcine the powder obtained in step 2 at 800° C. for 2.5 h in a muffle furnace to further solidify the granulated powder, and remove it for later use after natural cooling;
[0088] Step 4: 400 parts of titanium-containing blast furnace slag with a titanium content of 17% are ground into particles with a particle size of 1 μm using a jet mill, based on 10 g per part;
[0089] Step 5: Weigh 30 parts of red mud solidified particles at 10 g each, weigh 3 parts of silica sol, place them in a three-dimensional mixer and mix for 30 minutes, then weigh 100 parts of titanium-containing blast furnace slag fine powder and place them in the mixer and mix for 20 minutes to obtain agglomerate particles.
[0090] Step 6: The obtained agglomerate particles are sintered at 650° C. for 2 h to solidify to obtain a catalyst.
[0091] Step 7: Weigh 10 parts of hydrogen peroxide solution (30%) and 17 parts of citric acid, stir for 3 minutes, and obtain an auxiliary agent.
[0092] Step 7: Add 80g of catalyst to 2kg of printing and dyeing wastewater, add 10g of auxiliary agent and 3.8g of ozone at the same time, maintain the water temperature at 25°C, and measure the COD and heavy metal content in the water after 35 minutes of reaction.
[0093] Table 1 Comparison of the effect of catalysts in treating printing and dyeing wastewater in Examples 1 to 3 and Comparative Examples 1 to 3
[0094]
[0095] a: Refer to "Surface Water Environmental Quality Standard" GB3838-2002.
Claims
1. A method for preparing an organic matter degradation catalyst having heavy metal adsorption function, Features: The red mud is dealkalized, granulated I and sintered I to obtain red mud solidified particles, and the red mud solidified particles and raw materials including steel slag and titanium-containing slag are granulated II and sintered II to obtain; wherein the total mass ratio of the red mud solidified particles to the titanium-containing slag and the steel slag is 15-30:60-100; the mass ratio of the titanium-containing slag to the steel slag is 40-60:20-40; the dealkalization process is: red mud is mixed with lime and water in a mass ratio of 1:(0.05-0.2):(1-3); the conditions of the sintering I are: sintering at a temperature of 800-900°C for 1-2.5h; the conditions of the sintering II are: sintering at a temperature of 550-650°C for 1-3h.
2. A method for preparing an organic matter degradation catalyst having heavy metal adsorption function according to claim 1, Features: The granulation I adopts spray granulation, and the particle size of the granules is controlled at 10-15 microns.
3. The method for preparing an organic matter degradation catalyst having heavy metal adsorption function according to claim 1, Features: The titanium content of the titanium-containing slag is greater than 15% by mass.
4. The method for preparing an organic matter degradation catalyst having heavy metal adsorption function according to claim 1, Features: The raw material further comprises silica sol, and the mass of the silica sol is 2-15% of the mass of the solidified red mud particles.
5. The method for preparing an organic matter degradation catalyst having heavy metal adsorption function according to claim 1, Features: The granulation II adopts a three-dimensional mixing granulation method.
6. An organic matter degradation catalyst with heavy metal adsorption function, Features: Obtained by the preparation method according to any one of claims 1 to 5.
7. The organic matter degradation catalyst having heavy metal adsorption function as claimed in claim 6, Features: Used for heavy metal adsorption and / or catalytic degradation of organic matter in water bodies.
8. The organic matter degradation catalyst having heavy metal adsorption function according to claim 7, Features: The catalyst is used in the process of catalyzing the degradation of organic matter, and auxiliary agents including hydrogen peroxide, citric acid and ozone are added.
Citation Information
Patent Citations
Preparation of heat-treatment red mud catalyst and application thereof in water treatment technologies
CN103566959A
Method and application for preparing catalyst by using red mud as raw materials
CN105435795A
Preparation method and application of porous geological polymer microspheres
CN107973559A
Preparation method and application of red mud one-step synthetic magnetic adsorbent
CN109200991A
Method for preparing spherical granular adsorbent from Bayer process red mud and electrolytic manganese slag
CN111790348A