Method for extracting lithium from lepidolite using fluidized bed
Through fluidized bed technology, the high-temperature boiling and deep purification treatment of lithium mica is solved, and the problems of low lithium conversion rate and high accident rate in lithium mica extraction process are achieved, and efficient and safe lithium extraction of lithium mica is achieved, suitable for industrial production .
Patent Information
- Application Number
- CN202310004648.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-01-03
AI Technical Summary
In the existing lithium mica lithium extraction process, the lithium conversion rate and high accident rate are low during the high-temperature roasting process of rotary kilns and tunnel kilns, resulting in low lithium conversion rate and high accident rate, making it impossible to achieve industrialization and industrial production.
Using fluidized bed technology, the mixture of lithium mica, potassium-sodium mixed salt, calcium sulfate and calcium carbonate is roasted in a boiling state. The leaching of dilute aqueous sulfuric acid solution, solid-liquid separation, countercurrent washing and deep purification are obtained to obtain high-purity lithium. Solution.
It has achieved efficient extraction of lithium in lithium mica, with safe, stable and continuous process, low production cost, suitable for industrial and industrial production, and has improved the extraction rate of lithium to reach more than 90%.
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium material processing, and in particular to a method for extracting lithium from lithium mica using a fluidized bed. Background Art
[0002] At present, there are mainly lime roasting method, sulfate method, sulfuric acid method, chlorination method and pressure cooking method for extracting lithium from lithium mica to prepare lithium carbonate. However, the mainstream method for extracting lithium from lithium mica is sulfate method, and the equipment used is rotary kiln and tunnel kiln. After the process technology route is characterized, during the high-temperature roasting process of the rotary kiln, the potassium and sodium salt materials are added. Due to uneven heating during the rotation of the rotary kiln, ring formation and kiln formation occur, and the lithium conversion rate is low, and the yield is not high, about 65%. The tunnel kiln is a grafting technology for the roasting of red bricks of building materials. After the lithium mica and auxiliary materials are mixed, the press is pressed into bricks, and the stack is loaded on the kiln car for high-temperature roasting. However, the chemical and physical properties of lithium mica itself are poor in plasticity and strength. Stacking too high is easy to collapse, causing kiln trampling, high accident rate, and cannot be industrialized and industrialized. Summary of the invention
[0003] The purpose of the present application is to provide a method for extracting lithium from lepidolite using a fluidized bed to solve the above problems.
[0004] To achieve the above objectives, this application adopts the following technical solutions:
[0005] A method for extracting lithium from lepidolite using a fluidized bed, comprising:
[0006] Mixing raw materials including lepidolite, potassium-sodium mixed salt, calcium sulfate and calcium carbonate to obtain a mixture, aging the mixture and then feeding it into a fluidized bed, and roasting it in a boiling state to obtain a clinker;
[0007] The clinker is mixed with water and ball-milled, and then leached with a dilute sulfuric acid aqueous solution to obtain a lithium sulfate solid-liquid mixture; the lithium sulfate solid-liquid mixture is subjected to a first solid-liquid separation to obtain a leached residue and a leached liquid;
[0008] The leached residue is subjected to countercurrent washing, the washing liquid is combined with the leached liquid, and concentrated to obtain a lithium production solution, the pH of the lithium production solution is adjusted to a strong alkaline state, and then EDTA and a sodium carbonate aqueous solution are added to react, and the reaction product is subjected to a second solid-liquid separation to obtain a preliminary lithium solution and a filter residue;
[0009] The preliminary lithium solution is purified to obtain a refined lithium solution, and the filter residue is returned to the fluidized bed for circulation treatment.
[0010] Preferably, the mass ratio of the lepidolite, the potassium-sodium mixed salt, the calcium sulfate and the calcium carbonate is 60:15:15:10.
[0011] Preferably, the water content of the mixture is less than or equal to 2wt%, and the proportion of 40-60 mesh particles is not less than 80%.
[0012] Preferably, the aging temperature is 20-30°C and the time is not less than 24 hours.
[0013] Preferably, the fluidized bed uses water gas as fuel;
[0014] Preferably, the furnace outlet temperature of the fluidized bed is 860°C-900°C, and the temperature on both sides of the pneumatic distribution valve is 850°C-860°C.
[0015] Preferably, the mass ratio of the clinker to the water is (1-1.5):(2-3);
[0016] Preferably, the pH of the dilute sulfuric acid aqueous solution during leaching is 5-6, the temperature is room temperature, and the leaching time is 1h-2h.
[0017] Preferably, the lithium content in the leached residue after the countercurrent washing is less than or equal to 0.1wt%;
[0018] Preferably, the leached residue after the countercurrent washing is used as a concrete admixture.
[0019] Preferably, the pH corresponding to the strong alkalinity is not less than 12;
[0020] Preferably, the reaction time is 30 min and the temperature is 90°C.
[0021] Preferably, the concentration of the sodium carbonate aqueous solution is 170-189 g / L;
[0022] Preferably, the amount of the sodium carbonate aqueous solution is 1-2 times the theoretical value, and the amount of EDTA is 1-2 times the theoretical value.
[0023] Preferably, the purification is carried out using a battery-grade chelating resin tower;
[0024] Preferably, the contents of calcium and magnesium ions in the refined lithium production solution are both less than or equal to 2 ppm;
[0025] Preferably, the lithium ion content in the refined lithium-producing solution is not less than 12 g / L; when the lithium ion content is less than 12 g / L, the solution is returned to the concentration step.
[0026] Compared with the prior art, the beneficial effects of this application include:
[0027] The method for extracting lithium from lithium mica using a fluidized bed provided in the present application is to feed a mixture including lithium mica, potassium-sodium mixed salt, calcium sulfate and calcium carbonate into a fluidized bed after aging, and roast it in a boiling state, so that the lithium mica and potassium-sodium mixed salt, calcium sulfate, calcium carbonate and other auxiliary materials are in a high-temperature boiling state, and the ion decomposition and exchange are more sufficient, and it has the characteristics of simple operation, large adjustment range, good control performance, and low production cost. The whole process can achieve safe, stable, continuous and economical operation. The method obtains a refined lithium solution through mixing, aging, fluidized bed roasting, ball milling leaching, solid-liquid separation, purification and impurity removal of leached residue, and secondary deep purification of the preliminary lithium solution. The process is short, the operation is simple, and it is easy to industrialize and industrialize production; the refined lithium solution can be used as a raw material for preparing battery-grade lithium carbonate and battery-grade lithium hydroxide. DETAILED DESCRIPTION
[0028] As used herein:
[0029] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0030] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0031] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0032] In these examples, parts and percentages are by mass unless otherwise indicated.
[0033] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0034] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0035] A method for extracting lithium from lepidolite using a fluidized bed, comprising:
[0036] Mixing raw materials including lepidolite, potassium-sodium mixed salt, calcium sulfate and calcium carbonate to obtain a mixture, aging the mixture and then feeding it into a fluidized bed, and roasting it in a boiling state to obtain a clinker;
[0037] The clinker is mixed with water and ball-milled, and then leached with a dilute sulfuric acid aqueous solution to obtain a lithium sulfate solid-liquid mixture; the lithium sulfate solid-liquid mixture is subjected to a first solid-liquid separation to obtain a leached residue and a leached liquid;
[0038] The leached residue is subjected to countercurrent washing, the washing liquid is combined with the leached liquid, and concentrated to obtain a lithium production solution, the pH of the lithium production solution is adjusted to a strong alkaline state, and then EDTA and a sodium carbonate aqueous solution are added to react, and the reaction product is subjected to a second solid-liquid separation to obtain a preliminary lithium solution and a filter residue;
[0039] The preliminary lithium solution is purified to obtain a refined lithium solution, and the filter residue is returned to the fluidized bed for circulation treatment.
[0040] The reaction mechanism is as follows:
[0041] 1.Li2O·Al2O3·8SiO2+CaSO4→CaO·Al2O3·8SiO2+Li2SO4 (850-860℃);
[0042] 2.Li2O·Al2O3·8SiO2+Na2SO4→Na2O·Al2O3·8SiO2+Li2SO4 (850-860℃);
[0043] 3.Li2O·Al2O3·8SiO2+K2SO4→K2O·Al2O3·8SiO2+Li2SO4 (850-860℃);
[0044] 3.2F+Ca→CaF2 (solid fluorine).
[0045] Fluidized bed fluidized roasting technology is a process in which the valuable metal ions in lithium mica and the calcium, sodium, and potassium ions in the auxiliary materials are in the boiling ground state. The contact time between the ions is long, the contact area between the ions is large, and the ions are fully combined and reacted to form soluble sulfuric acid system salts (lithium, potassium, sodium, rubidium, and cesium), which can be efficiently extracted, providing convenience for subsequent metal separation.
[0046] In an optional embodiment, the mass ratio of the lepidolite, the potassium-sodium mixed salt, the calcium sulfate and the calcium carbonate is 60:15:15:10.
[0047] In an optional embodiment, the water content of the mixture is less than or equal to 2wt%, and the proportion of 40-60 mesh particles is not less than 80%.
[0048] Optionally, the moisture content of the mixture can be 0.1%, 0.5%, 1%, 1.5%, 2% or any value less than or equal to 2wt%, and the proportion of 40-60 mesh particles can be 80%, 85%, 90%, 95% or any value not less than 80%.
[0049] In an optional embodiment, the aging temperature is 20-30°C and the time is not less than 24 hours.
[0050] Optionally, the aging temperature may be 20°C, 25°C, 30°C or any value between 20-30°C.
[0051] In an optional embodiment, the fluidized bed uses water gas as fuel;
[0052] In an optional embodiment, the furnace outlet temperature of the fluidized bed is 860°C-900°C, and the temperature on both sides of the pneumatic distribution valve is 850°C-860°C.
[0053] Optionally, the furnace outlet temperature of the fluidized bed can be 860℃, 870℃, 880℃, 890℃, 900℃ or any value between 860℃-900℃, and the temperature on both sides of the pneumatic distribution valve can be 850, 855, 860 or any value between 850℃-860℃.
[0054] In an optional embodiment, the mass ratio of the clinker to the water is (1-1.5):(2-3);
[0055] In an optional embodiment, the pH of the dilute sulfuric acid aqueous solution is 5-6, the temperature is room temperature, and the time is 1h-2h.
[0056] Optionally, the mass ratio of the clinker to the water can be 1:2, 1:2.5, 1:3, 1.5:2, 1.2:2.5, 1.2:3 or any value between (1-1.5):(2-3); the pH of the leaching of the dilute sulfuric acid aqueous solution can be 5, 5.5, 6 or any value between 5-6, the temperature is room temperature, and the time can be 1h, 1.5h, 2h or any value between 1h-2h.
[0057] In an optional embodiment, the lithium content in the leached residue after the countercurrent washing is less than or equal to 0.1wt%;
[0058] In an optional embodiment, the leached residue after the countercurrent washing is used as a concrete admixture.
[0059] In an optional embodiment, the pH corresponding to the strong alkalinity is not less than 12;
[0060] In an optional embodiment, the reaction time is 30 minutes and the temperature is 90°C.
[0061] In an optional embodiment, the concentration of the sodium carbonate aqueous solution is 170-189 g / L;
[0062] Optionally, the concentration of the sodium carbonate aqueous solution may be 170 g / L, 175 g / L, 180 g / L, 185 g / L, 189 g / L or any value between 170 and 189 g / L;
[0063] In an optional embodiment, the amount of the sodium carbonate aqueous solution is 1-2 times the theoretical value, and the amount of EDTA is 1-2 times the theoretical value.
[0064] Optionally, the dosage of the sodium carbonate aqueous solution can be 1 times, 1.5 times, 2 times or any value between 1-2 times the theoretical value, and the dosage of the EDTA can be 1 times, 1.5 times, 2 times or any value between 1-2 times the theoretical value.
[0065] In an optional embodiment, the purification is performed using a battery-grade chelating resin tower;
[0066] In an optional embodiment, in the refined lithium production solution, the contents of calcium and magnesium ions are both less than or equal to 2 ppm;
[0067] In an optional embodiment, the lithium ion content in the refined lithium-producing solution is not less than 12 g / L; when the lithium ion content is less than 12 g / L, the solution is returned to the concentration step.
[0068] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0069] Example 1
[0070] This embodiment provides a method for extracting lithium from lepidolite using a fluidized bed, which specifically comprises the following steps:
[0071] According to the mass ratio, lithium mica: potassium and sodium sulfate system mixed salt: calcium sulfate: calcium carbonate = 60:20:15:5 are mixed. The potassium and sodium mixed salt belongs to Jinhui's self-produced salt, and calcium sulfate and calcium carbonate belong to industrial grade. The appearance of calcium carbonate and calcium sulfate is finely divided. The materials are mixed by a high-efficiency spiral mixer for 30 minutes. The moisture content of the mixture is 1.5%, and the particle size distribution is 55 mesh. The proportion is 85.6%. The mixed material is conveyed to the high-temperature silo by belt conveyor, aged for 26 hours, and the mixed material is pre-treated and activated. With water gas as the fuel carrier, the lithium mica mixture is sent to the inlet of the air preheater. The mixture forms a boiling ground state in the fluidized bed reaction roaster. The materials are fully roasted at high temperature, and the ion exchange reaction is thorough, ensuring that the furnace outlet temperature is 880℃, and the temperature on both sides of the pneumatic distribution valve is controlled at 860℃, and the operation is stable. The roasted clinker is fully ball-milled with water, and the pH is adjusted to 5 with dilute sulfuric acid, and the leaching water washing treatment is carried out. The soluble lithium ions in the finely milled material are fully leached to form a solid-liquid mixture of lithium sulfate salt. The mass ratio of the roasted fine powder and water is controlled to be 1:2, the temperature of the leaching water is room temperature, and the water leaching time is 1h. The solid-liquid mixture of lithium sulfate is separated into solid and liquid by a filtering device to obtain a filter residue and a filtrate, and the filter residue can be a concrete admixture. The leached residue is washed 4 times in countercurrent, and the filtering device is a combination of a belt filter and a plate and frame filter press, and the lithium ion concentration in the lithium residue is controlled to be 0.9wt%; the filtrate and washing liquid prepared above are mixed together to form a lithium solution, and the lithium solution is evaporated and concentrated to obtain a lithium solution. In order to obtain a qualified refined lithium solution, an appropriate amount of sodium hydroxide is added to the lithium solution to adjust the alkalinity to 12.78, 1.5 times the theoretical value of EDTA and a small amount of sodium carbonate with a concentration of 185g / L solution, and the reaction is carried out for 30min at a reaction temperature of 90°C. Use plate and frame filter press to separate solid and liquid, remove impurities Ca 2+ Mg 2+ , Fe 3+ , Mn 2+ 、F - 、Al 3+ The filtrate is the preliminary lithium solution. The filter residue is returned to the previous fluidized bed for calcination and reuse. The preliminary lithium solution in the previous step is deeply purified and impurities removed through a battery-grade chelating resin tower.2+ Mg 2+ Remove and purify the solution Ca 2+ Mg 2+ The ion mass concentration is 2ppm. Battery-grade chelating resin can be recycled after dilute hydrochloric acid analysis. The lithium ion mass concentration is 13.55g / L. The refined lithium liquid becomes the raw material for the subsequent lithium precipitation module to prepare battery-grade lithium carbonate and battery-grade lithium hydroxide. From a practical point of view, the current fluidized bed fluidized bed technology is used to roast and extract lithium from lithium mica, with a high production operation rate and continuous production. Achieve safe, stable, continuous and good operation status.
[0072] Example 2
[0073] This embodiment provides a method for extracting lithium from lepidolite using a fluidized bed, which specifically comprises the following steps:
[0074] According to the mass ratio, lithium mica: potassium and sodium sulfate system mixed salt: calcium sulfate: calcium carbonate = 65:15:10:10. The potassium and sodium mixed salt belongs to the self-produced salt of Penghui Recycling Technology Co., Ltd., and calcium sulfate and calcium carbonate belong to industrial grade. The appearance of calcium carbonate and calcium sulfate is finely divided. Mix the materials with a high-efficiency spiral mixer for 20 minutes, the moisture content of the mixture is 2%, and the particle size distribution is 60 mesh. The proportion is 70.6%. The mixture is conveyed to the high-level silo by belt conveyor, aged for 24 hours, and pre-treated and activated. With water gas as the fuel carrier, the lithium mica mixture is sent to the inlet of the air preheater. The mixture forms a boiling ground state in the fluidized bed reaction roaster. The materials are fully roasted at high temperature, and the ion exchange reaction is thorough, ensuring that the furnace outlet temperature is 880°C, and the temperature on both sides of the pneumatic distribution valve is controlled at 880°C, and the operation is stable. The roasted clinker is fully ball-milled with water, and the pH is adjusted to 5.5 with dilute sulfuric acid, and the leaching water washing treatment is carried out. The soluble lithium ions in the finely milled material are fully leached to form a solid-liquid mixture of lithium sulfate salt. The mass ratio of the roasted fine powder and water is controlled to be 1:1.5, the temperature of the leaching water is room temperature, and the water leaching time is 1h. The solid-liquid mixture of lithium sulfate is separated into solid and liquid by a filtering device to obtain a filter residue and a filtrate, and the filter residue can be a concrete admixture. The leached residue is washed twice in countercurrent, and the filtering device is a combination of a belt filter and a plate and frame filter press, and the lithium ion concentration in the lithium residue is controlled to be 0.9wt%; the filtrate and washing liquid prepared above are mixed together to form a lithium solution, and the lithium solution is evaporated and concentrated to obtain a lithium solution. In order to obtain a qualified refined lithium solution, an appropriate amount of sodium hydroxide is added to the lithium solution to adjust the alkalinity to 12.00, 2 times the theoretical value of EDTA and a small amount of sodium carbonate The concentration is 170g / L solution, the reaction is carried out for 30min, and the reaction temperature is 80℃. Use plate and frame filter press to separate solid and liquid, remove impurities Ca 2+ Mg 2+ , Fe 3+ , Mn 2+ 、F -、Al 3+ The filtrate is the preliminary lithium solution. The filter residue is returned to the previous fluidized bed for calcination and reuse. The preliminary lithium solution in the previous step is deeply purified and impurities removed through a battery-grade chelating resin tower. 2+ Mg 2+ Remove and purify the solution Ca 2+ Mg 2+ The ion mass concentration is 5ppm. Battery-grade chelating resin can be recycled after dilute hydrochloric acid analysis. The lithium ion mass concentration is 13.55g / L. The refined lithium liquid becomes the raw material for the subsequent lithium precipitation module to prepare battery-grade lithium carbonate and battery-grade lithium hydroxide. From a practical point of view, the current fluidized bed fluidized bed technology is used to roast and extract lithium from lithium mica, with a high production operation rate and continuous production. Achieve safe, stable, continuous and good operation status.
[0075] Comparative Example 1
[0076] The difference from Example 1 is that the roasting method is different. Instead of using a fluidized bed, a rotary kiln is used. The other process parameters are controlled exactly the same, that is, the above-mentioned lithium mica mixture is also roasted in a rotary kiln. After testing, the lithium extraction rate is greatly reduced to less than 70%. The specific test data are shown in Table 1.
[0077] Comparative Example 2
[0078] The difference from Example 1 is that the roasting method is different. Instead of a fluidized bed, a tunnel kiln is used. The other process parameters are controlled exactly the same, that is, the above-mentioned lithium mica mixture is also roasted through a tunnel kiln. After testing, the lithium extraction rate is greatly reduced to less than 80%. The specific test data are shown in Table 1.
[0079] Table 3 below is a comparison table of the extraction rates of lithium and various valuable metal elements in Examples 1 and 2 and Comparative Examples 1 and 2 using the process of the present invention.
[0080] Table 1 Comparison of extraction rates of lithium and other valuable metals
[0081] name Lithium extraction rate Rubidium extraction rate Cesium extraction rate Potassium extraction rate Sodium extraction rate Comparative Example 1 65.26% 68.17% 69.94% 61.08% 62.56% Comparative Example 2 75.34% 60.29% 73.64% 72.04% 63.69% Example 1 91.22% 87.23% 88.14% 90.12% 90.46% Example 2 91.82% 88.79% 85.74% 90.93% 90.77%
[0082] Table 1 shows that the method provided by the present application has a greatly improved extraction rate of lithium and other metals in lithium mica clinker relative to conventional tunnel kilns and rotary kilns. By experimental comparison, other process methods are used, especially when the same existing preparation process method and technical parameters are controlled, and the above-mentioned material for roasting of the present invention is roasted in a rotary kiln, the highest extraction rate is less than 75%, and sometimes even less than 65%. By using the process method of the present application, the effective extraction rate of lithium in lithium mica clinker can reach more than 90%, so that the elements in the lithium mica clinker are efficiently extracted and recycled, and the economic benefits are greatly improved, realizing resource recycling.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0084] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for extracting lithium from lepidolite using a fluidized bed, characterized in that: include: Mix raw materials including lepidolite, potassium-sodium mixed salt, calcium sulfate and calcium carbonate to obtain a mixture, age the mixture, and then feed it into a fluidized bed, and roast it in a boiling state to obtain a clinker; the water content of the mixture is less than or equal to 2wt%, and the proportion of 40-60 mesh particles is not less than 80%; the aging temperature is 20-30°C, and the time is not less than 24h; the furnace outlet temperature of the fluidized bed is 860°C-900°C, and the temperature on both sides of the pneumatic distribution valve is 850°C-860°C; The clinker is mixed with water and then ball-milled, and then leached with a dilute sulfuric acid aqueous solution to obtain a lithium sulfate solid-liquid mixture; the lithium sulfate solid-liquid mixture is subjected to a first solid-liquid separation to obtain a leached residue and a leached liquid; the mass ratio of the clinker to the water is (1-1.5): (2-3); the pH of the dilute sulfuric acid aqueous solution is 5-6, the temperature is room temperature, and the time is 1h-2h; The leached residue is subjected to countercurrent washing, and the washing liquid is combined with the leached liquid and concentrated to obtain a lithium production solution, the pH of the lithium production solution is adjusted to a strong alkaline state, and then EDTA and an aqueous sodium carbonate solution are added to react, and the reaction product is subjected to a second solid-liquid separation to obtain a preliminary lithium solution and a filter residue; the pH corresponding to the strong alkalinity is not less than 12; the concentration of the aqueous sodium carbonate solution is 170-189 g / L, the amount of the aqueous sodium carbonate solution is 1-2 times the theoretical value, and the amount of EDTA is 1-2 times the theoretical value; The preliminary lithium solution is purified to obtain a refined lithium solution, and the filter residue is returned to the fluidized bed for circulation treatment.
2. The method according to claim 1, characterized in that: The mass ratio of the lepidolite, the potassium-sodium mixed salt, the calcium sulfate and the calcium carbonate is 60:15:15:
10.
3. The method according to claim 1, characterized in that The fluidized bed uses water gas as fuel.
4. The method according to claim 1, characterized in that: The lithium content in the leached residue after the countercurrent washing is less than or equal to 0.1wt%.
5. The method according to claim 1, characterized in that The leached residue after the countercurrent washing is used as a concrete admixture.
6. The method according to claim 1, characterized in that The reaction time is 30 minutes and the temperature is 90°C.
7. The method according to any one of claims 1 to 6, characterized in that: The purification is carried out using a battery-grade chelating resin tower.
8. The method according to any one of claims 1 to 6, characterized in that: In the refined lithium production solution, the contents of calcium and magnesium ions are both less than or equal to 2 ppm.
9. The method according to any one of claims 1 to 6, characterized in that: The lithium ion content in the refined lithium-producing solution is not less than 12 g / L; when the lithium ion content is less than 12 g / L, the solution is returned to the concentration step.
Citation Information
Patent Citations
Process of producing lithium carbonate
CA1297265C
Process for preparing lithium carbonate from lepidolite by novel sulfate roasting method
CN113636579A
Method for extracting lithium from lithium chinastone mineral by roasting with mixed sulfate method
CN113999970A