A highly adaptable ultrafine mineral admixture grinding aid activator and preparation method thereof
By using grinding excitants composed of triethanolamine, sulfate, calcium sulfaluminate, etc., the problem of insufficient adaptability of grinding excitants in the prior art is solved, and a high-activity and high-performance ultrafine mineral blend is realized , simplifies the preparation process and reduces costs.
Patent Information
- Application Number
- CN202210683762.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-06-16
AI Technical Summary
In the prior art, the grinding exciter is insufficiently adaptable to different types of ultrafine mineral blends, which leads to difficult engineering operations, complex preparation processes and high cost.
Using a high-adaptive ultrafine mineral blend of triethanolamine, sulfate, calcium sulfaluminate, lignin sulfonate, gypsum and styrene-maleic anhydride copolymer resin, grinding and stirring Preparation by heating to improve the specific surface area and activity of the blend.
It significantly improves the activity of the blend material and the mechanical properties of the concrete, reduces the difficulty of engineering operation and preparation cost, and is suitable for blend materials of different compositions and contents, simplifying the preparation process.
Smart Images

Figure BDA0003697270230000041 
Figure BDA0003697270230000042 
Figure BDA0003697270230000051
Abstract
Description
Technical Field
[0001] The present invention relates to a concrete additive, and in particular to a highly adaptable ultrafine mineral admixture grinding aid activator and a preparation method thereof. Background Art
[0002] In recent years, process residues such as steel slag, slag and fly ash have been widely used in the construction field. There are many reports on using steel slag, slag and fly ash as ultrafine mineral admixtures for the reinforcement of concrete materials. Since the amount of concrete materials used in the construction industry is very large, this is a good solution to the secondary utilization of waste, reducing production costs and environmental pollution. The premise of the secondary utilization of these waste materials and waste residues is that the admixtures need to be formed into ultrafine powders and only after grinding can they have high activity. Up to now, grinding aids are usually used to improve grinding efficiency and performance, thereby increasing production and various technical indicators.
[0003] Chinese patent CN101367631A discloses an activator in the preparation process of ultrafine fly ash-based composite mineral admixture, which is a mixture of 10 to 30 parts of polysaccharide, 10 to 30 parts of sodium acetate, 10 to 30 parts of alkanolamine and 10 to 70 parts of carrier water by weight. However, the activator is for ultrafine fly ash-based composite mineral admixture with a specific surface area of 1000m 2 / kg±100m 2 / kg of ultrafine fly ash.
[0004] Chinese patent CN 111499294 A discloses that the grinding aid activator is composed of the following raw materials by weight: 10-20 parts of triethanolamine, 5-6 parts of sodium dodecylbenzene sulfonate, 2-3 parts of acrylic acid glycidyl ether, 3-5 parts of polyaluminium iron silicate, 10-15 parts of sodium silicate, 5-10 parts of magnesium hexafluorosilicate, and the rest is water. The specific surface area of the ultrafine powder selected by the ultrafine air separation system is 900m 2 / kg.
[0005] Chinese patent CN 112299748 A discloses a high-activity ultrafine concrete admixture grinding aid activator, characterized in that it is composed of the following raw materials in parts by weight: 20 to 25 parts of sodium sulfate, 8 to 12 parts of sodium silicate, 4 to 6 parts of sodium fluorosilicate, 5 to 7 parts of nano magnesium aluminum silicate, 5 to 7 parts of sodium carbonate, 6 to 9 parts of sodium sulfate, 2 to 3 parts of sodium hexametaphosphate, 4 to 7 parts of epoxidized butyl oleate, 3 to 5 parts of acetyl tributyl citrate, 1.8 to 2.5 parts of acetylic acid methyl ester, 2.8 to 3.6 parts of calcium lignin sulfonate, 2.0 to 2.5 parts of magnesium sulfate, 3.6 to 4.8 parts of coconut oil diethanolamide, 4.8 to 5.6 parts of vinyl triethoxysilane, 6.2 to 7.5 parts of triethanolamine, 4.5 to 6.2 parts of sodium dodecyl sulfate, 12 to 16 parts of polymer dispersant and 450 to 500 parts of ultrapure water. However, the components of the grinding aid activator are too complex and require a special polymer dispersant for preparation. In addition, the preparation method of the grinding aid activator is also complicated and requires multiple chemical reactions.
[0006] Although there are many studies in the prior art, and although admixtures with higher activity can be obtained, they are not adaptable to different types of admixtures and need to find suitable grinding aids, which is not conducive to actual engineering operations. Summary of the invention
[0007] In view of the defects and needs in the prior art, the purpose of the present invention is to provide a highly adaptable ultrafine mineral admixture grinding aid activator and a preparation method thereof. The grinding aid activator prepared by the present invention can improve the activity of the admixture, thereby improving the relevant mechanical properties of ultra-high performance concrete; and has good adaptability to different types of industrial waste, greatly reducing the difficulty of engineering operations.
[0008] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a highly adaptable ultrafine mineral admixture grinding aid activator, composed of the following raw materials in parts by weight: 30-50 parts of triethanolamine, 25-30 parts of sulfate, 10-20 parts of calcium sulfoaluminate, 5-10 parts of lignin sulfonate, 5-10 parts of gypsum, 5-10 parts of polyether ester of styrene-maleic anhydride copolymer resin, 1-5 parts of lauryl alcohol polyoxyethylene ether, and 300-400 parts of water.
[0009] Furthermore, a highly adaptable ultrafine mineral admixture grinding aid activator is composed of the following raw materials in parts by weight: 35-45 parts of triethanolamine, 27-28 parts of sulfate, 14-16 parts of calcium sulfoaluminate, 7-8 parts of lignin sulfonate, 6-8 parts of gypsum, 6-9 parts of polyether ester of styrene-maleic anhydride copolymer resin, 2-3 parts of lauryl alcohol polyoxyethylene ether, and 320-380 parts of water.
[0010] Furthermore, the gypsum is selected from one or more of hemihydrate gypsum, dihydrate gypsum or natural anhydrite.
[0011] Furthermore, the sulfate is selected from one or more of sodium sulfate, magnesium sulfate and calcium sulfate.
[0012] Furthermore, the lignin sulfonate is selected from one or more of sodium lignin sulfonate and calcium lignin sulfonate.
[0013] A method for preparing a highly adaptable ultrafine mineral admixture grinding aid activator comprises the following steps:
[0014] (1) Mix sulfate, calcium sulfoaluminate and gypsum evenly according to the ratio and grind until the specific surface area is greater than 500m 2 / Kg of mixed powder;
[0015] (2) placing water in a container, adding triethanolamine, lignin sulfonate, polyether ester of styrene-maleic anhydride copolymer resin and lauryl alcohol polyoxyethylene ether according to the proportion, stirring and heating to 40-50° C.;
[0016] (3) Adding the mixed powder in step (1) to step (2) in batches, stirring continuously during the adding process, to obtain a highly adaptable ultrafine mineral admixture grinding aid activator.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The grinding aid activator provided by the present invention can greatly increase the specific surface area of the admixture powder, thereby obtaining ultrafine mineral admixtures and improving their activity, thereby further ensuring the improvement of the mechanical properties of ultra-high performance concrete.
[0019] (2) The grinding aid activator provided by the present invention can grind admixtures of different compositions and contents and has good adaptability. It has great advantages in actual engineering, and there is no need to seek the corresponding grinding aid activator according to the composition of the admixture, which is more suitable for engineering operations.
[0020] (3) The grinding aid activator provided by the present invention does not require a complicated preparation process, saves the control of reaction process parameters, and greatly reduces the preparation cost. DETAILED DESCRIPTION
[0021] In order to enable those skilled in the art to better understand the technical solutions in the present application, the present invention is further described below in conjunction with embodiments. The described embodiments are only preferred embodiments of the present application, not all, and the present invention is not limited to the following embodiments.
[0022] Example 1
[0023] A highly adaptable ultrafine mineral admixture grinding aid activator is composed of the following raw materials in parts by weight: 30 parts of triethanolamine, 25 parts of calcium sulfate, 10 parts of calcium sulfoaluminate, 5 parts of sodium lignin sulfonate, 5 parts of hemihydrate gypsum, 5 parts of polyether ester of styrene-maleic anhydride copolymer resin, 1 part of lauryl alcohol polyoxyethylene ether, and 300 parts of water.
[0024] A method for preparing a highly adaptable ultrafine mineral admixture grinding aid activator comprises the following steps:
[0025] (1) Mix calcium sulfate, calcium sulfoaluminate and gypsum evenly according to the ratio and grind until the specific surface area is greater than 500m 2 / Kg of mixed powder;
[0026] (2) placing water in a container, adding triethanolamine, sodium lignin sulfonate, polyether ester of styrene-maleic anhydride copolymer resin and lauryl alcohol polyoxyethylene ether according to the ratio, stirring and heating to 40° C.;
[0027] (3) Adding the mixed powder in step (1) to step (2) in batches, stirring continuously during the adding process, to obtain a highly adaptable ultrafine mineral admixture grinding aid activator.
[0028] Example 2
[0029] A highly adaptable ultrafine mineral admixture grinding aid activator is composed of the following raw materials in parts by weight: 50 parts of triethanolamine, 30 parts of magnesium sulfate, 20 parts of calcium sulfoaluminate, 10 parts of calcium lignin sulfonate, 10 parts of natural anhydrite, 10 parts of polyether ester of styrene-maleic anhydride copolymer resin, 5 parts of lauryl alcohol polyoxyethylene ether, and 400 parts of water.
[0030] A method for preparing a highly adaptable ultrafine mineral admixture grinding aid activator comprises the following steps:
[0031] (1) Mix magnesium sulfate, calcium sulfoaluminate and gypsum evenly according to the ratio and grind until the specific surface area is greater than 500m 2 / Kg of mixed powder;
[0032] (2) placing water in a container, adding triethanolamine, calcium lignin sulfonate, polyether ester of styrene-maleic anhydride copolymer resin and lauryl alcohol polyoxyethylene ether according to the ratio, stirring and heating to 50° C.;
[0033] (3) Adding the mixed powder in step (1) to step (2) in batches, stirring continuously during the adding process, to obtain a highly adaptable ultrafine mineral admixture grinding aid activator.
[0034] Example 3
[0035] A highly adaptable ultrafine mineral admixture grinding aid activator is composed of the following raw materials in parts by weight: 40 parts of triethanolamine, 27 parts of sodium sulfate, 15 parts of calcium sulfoaluminate, 8 parts of sodium lignin sulfonate, 6 parts of dihydrate gypsum, 7 parts of polyether ester of styrene-maleic anhydride copolymer resin, 3 parts of lauryl alcohol polyoxyethylene ether, and 350 parts of water.
[0036] A method for preparing a highly adaptable ultrafine mineral admixture grinding aid activator comprises the following steps:
[0037] (1) Mix sodium sulfate, calcium sulfoaluminate and gypsum evenly according to the ratio and grind until the specific surface area is greater than 500m 2 / Kg of mixed powder;
[0038] (2) placing water in a container, adding triethanolamine, sodium lignin sulfonate, polyether ester of styrene-maleic anhydride copolymer resin and lauryl alcohol polyoxyethylene ether according to the proportion, stirring and heating to 45° C.;
[0039] (3) Adding the mixed powder in step (1) to step (2) in batches, stirring continuously during the adding process, to obtain a highly adaptable ultrafine mineral admixture grinding aid activator.
[0040] 1. Grinding performance test
[0041] In order to test the adaptability performance of grinding aid activator, this application provides three compositions of admixtures. 1. Composed of 50% slag, 30% steel slag, and 20% fly ash; 2. Composed of 50% water-quenched manganese slag, 30% slag, and 20% limestone; 3. Composed of 50% fly ash, 20% steel slag, and 20% slag. The specific grinding steps are: at the beginning of the grinding process, add 0.05% of the weight of the admixture to the admixture in three times, and the addition time is completed within 10 minutes. Record the performance of the admixtures at different grinding times. The specific results are recorded in Tables 1-3 respectively.
[0042] We also prepared the corresponding exciter as comparative example 1 according to Example 1 in patent CN101367631A; and prepared the corresponding exciter as comparative example 2 according to Example 1 in patent CN 111499294A.
[0043] Table 1: The admixture consists of 50% slag, 30% steel slag, and 20% fly ash.
[0044]
[0045] Table 2: The admixture consists of 50% water-quenched manganese slag, 30% slag, and 20% limestone.
[0046]
[0047] Table 3: The admixture consists of 50% fly ash, 20% steel slag, and 20% furnace slag.
[0048]
[0049] It can be seen from the data in Tables 1-3 that the grinding aid activator prepared by the present invention can significantly shorten the grinding time, and can obtain ultrafine mineral admixtures with a high specific surface area, thereby improving the activity. Most importantly, the present application can achieve good grinding aid effects for three admixtures with different compositions and contents. The activator in patent CN101367631A has a good effect on an admixture composed of 50% fly ash, 20% steel slag, and 20% furnace slag. Its grinding time is correspondingly shortened, and a higher powder specific surface area and activity are obtained. However, for the other two admixtures, its effect is obviously not as good as the grinding aid activator of the present application. The corresponding activator in patent CN 111499294A has a grinding time of 75min and a powder specific surface area of 826m for an admixture composed of 50% fly ash, 20% steel slag, and 20% furnace slag. 2 / kg, 28d activity index is 99.7; its performance is different from that of Examples 1-3 of the present application, but is basically at the same level. However, the effects of the other two admixtures are significantly reduced.
[0050] From the above comparison, it can be seen that the grinding aid activator of the present invention can obtain 900-1100m 2 / kg specific surface area of highly active, ultra-fine admixtures; and has good adaptability to admixtures of different compositions and contents.
[0051] 2. Mechanical properties test
[0052] We use a weight ratio of 52.5 grade ordinary Portland cement: quartz sand: admixture: water = 250:200:120:100 to form a concrete slurry, during which an appropriate amount of polycarboxylic acid water reducer is added; the test block is placed in a molding mold for curing to prepare. Note: The admixtures are respectively composed of 50% slag, 30% steel slag, and 20% fly ash, which are ground with grinding aids and activators in Example 1-3 and Comparative Example 1-2. Mechanical related tests are carried out according to GB / T 50080-2016 "Standard for Test Methods of Ordinary Concrete Mixture Performance", GB / T 0081-2016 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete" and GB / T50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete". The results are recorded in Table 4.
[0053] Table 4
[0054]
[0055]
[0056] From the results in Table 4, it can be seen that the high-activity admixture obtained by grinding with a grinding aid activator is used to prepare ultra-high performance concrete. The high-activity admixture plays a dense filling role as a filling material. Based on the close packing principle, it partially replaces cement and expensive raw materials, which can reduce the preparation cost of ultra-high performance concrete, and at the same time increase the added value of industrial solid waste, and effectively improve the working performance and mechanical properties of concrete. According to the data of the comparative example, it can be seen that different grinding aid activators have obvious differences in the activity of admixtures. Compared with the existing grinding aid activators, the present invention can obtain ultra-fine admixtures with larger specific surface area and higher activity, which is ultimately reflected in the improvement of the mechanical properties of concrete.
[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A highly adaptable ultrafine mineral admixture grinding aid activator, Features: The invention is composed of the following raw materials in parts by weight: 30-50 parts of triethanolamine, 25-30 parts of sulfate, 10-20 parts of calcium sulfoaluminate, 5-10 parts of lignin sulfonate, 5-10 parts of gypsum, 5-10 parts of polyether ester of styrene-maleic anhydride copolymer resin, 1-5 parts of lauryl alcohol polyoxyethylene ether, and 300-400 parts of water; The gypsum is selected from one or more of hemihydrate gypsum, dihydrate gypsum or natural anhydrite; The sulfate is selected from one or more of sodium sulfate, magnesium sulfate and calcium sulfate; The lignin sulfonate is selected from one or more of sodium lignin sulfonate and calcium lignin sulfonate.
2. According to claim 1, the highly adaptable ultrafine mineral admixture grinding aid activator, Features: The grinding aid activator is composed of the following raw materials in parts by weight: 35-45 parts of triethanolamine, 27-28 parts of sulfate, 14-16 parts of calcium sulfoaluminate, 7-8 parts of lignin sulfonate, 6-8 parts of gypsum, 6-9 parts of polyether ester of styrene-maleic anhydride copolymer resin, 2-3 parts of lauryl alcohol polyoxyethylene ether, and 320-380 parts of water.
3. A method for preparing the highly adaptable ultrafine mineral admixture grinding aid activator as claimed in any one of claims 1 to 2, Features: The following steps are involved: (1) mixing sulfate, calcium sulfoaluminate and gypsum uniformly according to the ratio, and grinding them into a mixed powder with a specific surface area greater than 500m2 / kg; (2) placing water in a container, adding triethanolamine, lignin sulfonate, polyether ester of styrene-maleic anhydride copolymer resin and lauryl alcohol polyoxyethylene ether according to the proportion, stirring and heating to 40-50° C.; (3) Adding the mixed powder in step (1) to step (2) in batches, stirring continuously during the adding process, to obtain a highly adaptable ultrafine mineral admixture grinding aid activator.