A chlorine removal composite material and its preparation method and application
By combining calcium-aluminum hydrotalcite with urban sludge to prepare chlorine removal composite materials, the existing chlorine removal methods are solved, and the existing chlorine removal methods are low-efficiency and environmentally friendly sludge landfill is achieved, and high-efficiency and low-cost chloride ion removal is achieved, with a wide range of Application value of water treatment.
Patent Information
- Application Number
- CN202211526691.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-30
AI Technical Summary
The existing chlorine removal methods have low efficiency and high energy consumption for high concentrations of chloride ions, and urban sludge landfill is not environmentally friendly, so we need to find a green and environmentally friendly treatment method.
Calcium-aluminum hydrotalcite is combined with urban sludge, and a chlorine removal composite material is prepared by calcination, which is used as an adsorbent for the removal of chloride ions in wastewater.
The chloride ion removal rate has been achieved above 70%, and the raw materials are easily obtained, low cost and high efficiency, and have great potential application value.
Smart Images

Figure CN115970641B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water treatment functional materials, and in particular to a chlorine removal composite material and a preparation method and application thereof. Background Art
[0002] Chloride ions in wastewater can cause great harm to the growth of crops. When the irrigation water contains high concentrations of chloride ions, it will affect the synthesis of protein in plants and lead to a large number of crop yield reductions. When the content is as high as 400mg﹒L -1 , which will cause the death of a large number of crops and vegetation. Chloride ions can also cause serious corrosion to metal industrial equipment. High concentrations of chloride ions are highly corrosive and can cause the passive film on the surface of metal materials to be destroyed and become soluble substances. As a result, the metal materials are partially corroded, which increases the cost of maintaining industrial equipment. At the same time, the damage to building materials is also great. When cement is produced in a high concentration of chloride ions, chlorides can enter the concrete through penetration or incorporation. The incorporation is because chloride salts are added during the production process of concrete. The penetration is due to the high chloride ion content in the atmosphere. Chloride ions diffuse through the concrete and the steel bar surface to the oxide thin film, destroying the passive film on the steel bar surface and causing electrochemical corrosion. In this process, the increase in solution concentration reduces the contact area with the air, thereby intensifying the oxidation reaction and accelerating the destructive effect of sulfate on the protective layer. Therefore, when the concrete structure is corroded, it must be repaired and reinforced in time. When the corrosion products rise, the pressure increases, and even causes the concrete to rupture, thereby reducing the life of the building. More importantly, it causes serious harm to humans and other organisms. The presence of high levels of chloride ions in the soil will lead to soil salinization and affect the growth of crops; excessive chloride ion content in drinking water will endanger human health, seriously affect heart, liver and kidney function, and lead to perchloric acid poisoning; in the ocean, excessive levels of chloride ions will increase the content of heavy metals in the water, affect the normal distribution of oxygen and the growth of nutrients, and thus make it impossible for seabed organisms to survive normally. Therefore, how to efficiently treat chlorine-containing wastewater has become an urgent issue to be solved. Some existing dechlorination methods mainly include precipitation, electrolysis, evaporation and concentration, ion exchange and electrosorption. Most of them have large process investments, high energy consumption, and unsatisfactory dechlorination efficiency.
[0003] Municipal sludge itself is a serious environmental pollution problem. Although it can be landfilled at present, the land area is constantly decreasing and it is not a long-term solution. Therefore, how to turn municipal sludge into treasure and use it to remove chlorine from chlorine-containing wastewater to achieve waste treatment is the technical problem to be solved by the present invention. Summary of the invention
[0004] In order to solve the above technical problems, a chlorine removal composite material and its preparation method and application are provided. The present invention combines calcium aluminum hydrotalcite with municipal sludge to form a composite material, which is used for wastewater dechlorination and has a good removal effect on chloride ions, and can be widely used for the removal of chloride ions in actual water samples.
[0005] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:
[0006] A method for preparing a chlorine removal composite material comprises the following steps:
[0007] (1) calcining calcium aluminum hydrotalcite (Ca-Al-LDHs) to obtain Ca-Al-LDO;
[0008] (2) calcining the dried municipal sludge in a protective atmosphere to obtain activated carbon material;
[0009] (3) The Ca-Al-LDO and the activated carbon material are uniformly mixed, dried, and calcined again to obtain a chlorine removal composite material.
[0010] Furthermore, the molar ratio of calcium to aluminum in the Ca-Al-LDHs is (1-5): 1, and preferably the molar ratio of calcium to aluminum in the Ca-Al-LDHs is (3-5): 1. A conventional preparation method is used.
[0011] Furthermore, in step 1, the calcination temperature of the Ca-Al-LDHs is 200-600°C for 4 hours, preferably the calcination temperature of the Ca-Al-LDHs is 500-600°C, and the most preferred calcination temperature of the Ca-Al-LDHs is 500°C.
[0012] Furthermore, in step 2, the calcination temperature of the municipal sludge is 200-700°C and the time is 3 hours. Preferably, the calcination temperature of the municipal sludge is 400-700°C, and most preferably, the calcination temperature of the municipal sludge is 500-600°C.
[0013] Furthermore, the calcination temperature in step 3 is 400-600° C. and the calcination time is 2 h.
[0014] Furthermore, in step 3, the mass ratio of Ca-Al-LDO to the activated carbon material is (1-5):1; preferably, the mass ratio of Ca-Al-LDO to the activated carbon material is (1-2):1.
[0015] Another aspect of the present invention provides a chlorine removal composite material obtained by the above preparation method, which is a composite of Ca-Al-LDO and activated carbon.
[0016] The last aspect of the present invention provides the use of the dechlorination composite material obtained by the above preparation method in dechlorination of wastewater. The dechlorination composite material is added to chlorine-containing wastewater at a dosage of 30-50g / L for dechlorination, and the chloride ion removal rate can reach more than 70%.
[0017] Beneficial technical effects:
[0018] The present invention calcines calcium aluminum hydrotalcite and municipal sludge to obtain Ca-Al-LDO and activated carbon materials respectively, mixes them as wet materials, and then dries and calcines them to obtain a Ca-Al-LDO-SS composite material, which is used as an adsorbent for dechlorination of wastewater to improve the removal rate of chloride ions. The method of the present invention has the advantages of easy raw material availability, green and environmental protection, low cost, high efficiency, good stability, etc., and has great potential application value in the field of water pollution treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The SEM image and element distribution diagram of the composite product Ca-Al-LDO-SS, which was prepared by combining Ca-Al-LDO-3-500 and SS-500 in a mass ratio of 2:1, before and after dechlorination.
[0020] Figure 2 This is a graph showing the change in chloride ion removal rate in wastewater over time with Ca-Al-LDO-3-500, SS-500 and the composite product Ca-Al-LDO-SS made from the two in a mass ratio of 2:1 at a feed rate of 40 g / L. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0022] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0023] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards; if there is no corresponding national standard, it is carried out according to the general international standards or the standard requirements proposed by relevant enterprises. Unless otherwise specified, all parts are by weight and all percentages are by weight.
[0024] Example 1
[0025] Preparation of Ca-Al-LDHs:
[0026] (1) Weigh 49.2 g of Ca(NO3)2 and 21.3 g of Al(NO3)3 (molar ratio of Ca:Al = 3:1) and dilute to a 250 mL volumetric flask with deionized water to obtain salt solution A;
[0027] (2) Add 1.7665 g Na2CO3 and 8 g NaOH to a 250 mL volumetric flask with deionized water to obtain a mixed alkaline solution B;
[0028] (3) While stirring vigorously with an electric stirrer, maintain the temperature of the electric heating mantle at 65°C, and simultaneously add salt solution A and mixed alkali solution B to a 500 mL three-necked flask. The titration endpoint is determined as the pH of the reaction system being 10±0.2. After reaching the titration endpoint, stop mixing the alkali solution B; maintain the temperature at 90°C for drying for 4 h, and then maintain the temperature at 80°C in a water bath for 6 h; filter and wash, and dry the filter cake in an oven at 80°C to obtain Ca-Al-LDHs.
[0029] The Ca-Al-LDHs with the above-mentioned molar ratio of Ca:Al=3:1 was placed in a crucible, sealed with tin foil, and calcined at 200°C, 300°C, 400°C, 500°C, and 600°C for 4 h, respectively, to obtain 5 samples Ca-Al-LDO, recorded as Ca-Al-LDO-3-200, Ca-Al-LDO-3-300, Ca-Al-LDO-3-400, Ca-Al-LDO-3-500, and Ca-Al-LDO-3-600.
[0030] Example 2
[0031] The dried municipal sludge was calcined in a tubular furnace with high-purity nitrogen protection during calcination. The calcinations were carried out at 200°C, 300°C, 400°C, 500°C, 600°C and 700°C for 3 h to obtain calcined sludge SS-activated carbon material samples, which were recorded as SS-200, SS-300, SS-400, SS-500, SS-600 and SS-700, respectively.
[0032] Example 3
[0033] A chlorine removal composite material and a preparation method thereof, comprising the following steps: mixing a series of Ca-Al-LDO of Example 1 and a series of sludge SS-activated carbon materials of Example 2 at a mass ratio of 2:1 in a single factor test, adding water to wet the materials and stirring and mixing for 4 hours, drying and calcining at 500° C. for 2 hours to obtain a series of chlorine removal composite materials represented by Ca-Al-LDO-SS. The specific chlorine removal performance of the composite materials is shown in Tables 1 and 2.
[0034] Example 4
[0035] Weigh 0.6585 g of NaCl and dilute it to 800 mg / L in a 500 mL volumetric flask with deionized water. -1 Chloride ion solution. Add 50mL, 800mg·L -1 2g of a series of Ca-Al-LDO-SS prepared in Example 3 were added to the chloride ion solution as a chloride ion adsorbent, and the reaction was stirred on a magnetic stirrer for 60 minutes. After centrifugation, 2mL of the upper clear liquid was aspirated with a pipette and diluted to a 10mL volumetric flask with deionized water. 2-3mL of the solution was aspirated with a syringe and filtered through a filter head and stored in a 5mL test tube. Weigh 0.38g of Na2CO3 (super pure) and diluted to a 1000mL volumetric flask with deionized water. After suction filtration, ultrasonicate for 10 minutes to obtain the eluent. Open the ion chromatograph, run the ultrapure water and eluent, and use an injection needle to draw the test solution in the test tube for injection to determine the Cl - The concentration of chloride ions was calculated using the following formula:
[0036] ,
[0037] Where C0 represents the initial concentration of chloride ions, and C represents the concentration of chloride ions after removal, mg﹒ L -1 . W represents the chloride ion removal rate, %.
[0038] The results are shown in Tables 1 and 2 below.
[0039] Table 1 Chloride ion removal rate of a series of Ca-Al-LDO-SS
[0040]
[0041]
[0042] It can be seen from Table 1 that under the single factor experimental variable, the composite product Ca-Al-LDO-SS obtained by mixing SS-500 with Ca-Al-LDO-3-500 and Ca-Al-LDO-3-600 in a mass ratio of 1:2 has a removal effect of more than 70% on chloride ions in wastewater.
[0043] Table 2 Chloride ion removal rate of a series of Ca-Al-LDO-SS
[0044]
[0045] As shown in Table 2, under the single factor test variable, the composite product Ca-Al-LDO-SS obtained by mixing Ca-Al-LDO-3-500 with SS-400, SS-500, SS-600 and SS-700 at a mass ratio of 2:1 has a removal effect of more than 70% on chloride ions in wastewater. More preferably, the composite product Ca-Al-LDO-SS obtained by mixing Ca-Al-LDO-3-500 with SS-500, SS-600 and SS-700 at a mass ratio of 2:1 has a removal effect of more than 73% on chloride ions in wastewater.
[0046] Example 5
[0047] The preparation of Ca-Al-LDHs in this embodiment is the same as that in Example 1, except that the molar ratio of Ca:Al in Ca-Al-LDHs is 1:1, Ca:Al=2:1, Ca:Al=3:1, Ca:Al=4:1, and Ca:Al=5:1, and they are calcined at 500°C for 4h to obtain a series of Ca-Al-LDO, which are respectively recorded as Ca-Al-LDO-1-500, Ca-Al-LDO-2-500, Ca-Al-LDO-3-500 (Example 1), Ca-Al-LDO-4-500, and Ca-Al-LDO-5-500. The above series of Ca-Al-LDO and SS-500 are mixed at a mass ratio of 2:1 and stirred for 4h, and then dried and calcined at 500°C for 2h to obtain a series of composite materials, represented by Ca-Al-LDO-SS, as shown in Table 3.
[0048] A series of Ca-Al-LDO-SS in this example was used to dechlorinate wastewater. The operation process was referred to Example 4. The specific results are shown in Table 3.
[0049] Table 3 Chloride ion removal rate of a series of Ca-Al-LDO-SS
[0050]
[0051]
[0052] It can be seen from Table 3 that under the single factor test variable, the composite product Ca-Al-LDO-SS prepared by the mass ratio of 2:1 of Ca-Al-LDO with a calcium-aluminum molar ratio of (3-4):1 calcined at 500°C and SS-activated carbon material calcined at 500°C has a removal effect of more than 75% on chloride ions in wastewater; more preferably, the composite product Ca-Al-LDO-SS prepared by the mass ratio of 2:1 of Ca-Al-LDO-3-500 and SS-500 can achieve a removal effect of more than 82% on chloride ions in wastewater.
[0053] Example 6
[0054] A series of composite products Ca-Al-LDO-SS were prepared by mixing Ca-Al-LDO-3-500 with SS-500 in different mass ratios of 1:1, 2:1, 3:1, 4:1 and 5:1, and used as chloride ion adsorbents to dechlorinate wastewater. The operation process was referred to Example 4, and the specific results are shown in Example 4.
[0055] Table 4 Effect of Ca-Al-LDO-SS, a composite product prepared by different mass ratios of Ca-Al-LDO-3-500 and SS-500, on dechlorination of wastewater
[0056]
[0057] As can be seen from Table 4, the chloride ion removal rate of the composite product Ca-Al-LDO-SS prepared by mixing Ca-Al-LDO-3-500 and SS-500 in a mass ratio of (1-5):1 in wastewater reaches more than 70%; among them, the chloride ion removal rate of the composite product Ca-Al-LDO-SS prepared by mixing Ca-Al-LDO-3-500 and SS-500 in a mass ratio of (1-2):1 in wastewater reaches more than 80%.
[0058] The composite product Ca-Al-LDO-SS prepared by Ca-Al-LDO-3-500 and SS-500 in a mass ratio of 2:1 was observed by SEM before and after dechlorination. The results are as follows Figure 1 As shown by Figure 1 It can be seen that the composite material Ca-Al-LDO-SS before and after dechlorination showed a lamellar structure, and the composite material before dechlorination showed a relatively regular hexagonal lamellar structure. It can be seen that more chloride ions were adsorbed in the composite material after dechlorination.
[0059] The removal rate of chloride ions from wastewater with time was investigated by using Ca-Al-LDO-3-500, SS-500 and the composite product Ca-Al-LDO-SS prepared by the mass ratio of the two at 2:1 with a feed amount of 40 g / L. Figure 2 As shown by Figure 2It can be seen that when the feed amount is 40g / L, the chloride ion removal rate of the three materials has almost no significant change after the reaction reaches 40min, indicating that each material basically reaches adsorption equilibrium after 40min of adsorption. The chloride ion removal rates of Ca-Al-LDO-3-500 alone or SS-500 alone in wastewater are about 52% and 42% respectively after 40min. The present invention uses Ca-Al-LDO-3-500 and SS-500 in a mass ratio of 2:1 to prepare the composite product Ca-Al-LDO-SS, which can achieve a chloride ion removal rate of 82% in wastewater after 40min. After the two form a composite material, they have a good removal rate of chloride ions. The reason for the high chloride ion removal rate may be that urban sludge contains elements such as nitrogen and phosphorus, as well as silicon, iron, calcium, and aluminum. During the calcination process, both inorganic and organic matter produce gases, and pores are generated on the sludge surface, thereby obtaining a porous, nitrogen- and phosphorus-doped activated carbon material with a large specific surface area. When the activated carbon material is mixed with calcined calcium aluminum hydrotalcite (Ca-Al-LDO) as a wet material, the surface hydroxyls of the two react to bond the calcined calcium aluminum hydrotalcite to the surface of the activated carbon material to form a composite material Ca-Al-LDO-SS. Due to the layered structure of Ca-Al-LDO and the porous nitrogen- and phosphorus-doped activated carbon material, the synergistic adsorption of chloride ions is produced, thereby improving the dechlorination performance of wastewater.
[0060] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. Application of the dechlorination composite material in wastewater dechlorination, characterized in that: The chlorine removal composite material is added to chlorine-containing wastewater at a dosage of 30-50 g / L for chlorine removal, and the chloride ion removal rate can reach more than 70%; The preparation method of the chlorine removal composite material comprises the following steps: (1) calcining calcium aluminum hydrotalcite to obtain Ca-Al-LDO; The molar ratio of calcium to aluminum in Ca-Al-LDHs is 3-5:1; The calcination temperature of Ca-Al-LDHs was 500-600°C and the time was 4 h; (2) calcining the dried municipal sludge in a protective atmosphere to obtain activated carbon material; The municipal sludge is calcined at a temperature of 400-700°C for 3 hours; (3) mixing the Ca-Al-LDO and the activated carbon material uniformly, drying them, and calcining them again to obtain a chlorine removal composite material; the calcination temperature in step 3 is 400-600° C. and the calcination time is 2 h; The mass ratio of the Ca-Al-LDO to the activated carbon material is 1-5:1.
Citation Information
Patent Citations
Sludge biochar loaded magnesium-iron oxide composite material for removing lead and cadmium in water as well as preparation method and application thereof
CN113634228A