Preparation method and application of graphene-ionic liquid composite sulfur adsorbent
Through the preparation of graphene-ionic liquid composite materials, the π-π stacking effect and the ionic liquid structure are used to solve the problem of difficult removal of thiophene macromolecule sulfides in liquid methane, and achieve efficient methane propellant purification with high adsorption efficiency. of traditional materials.
Patent Information
- Application Number
- CN202211075773.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-02
AI Technical Summary
Existing technology is difficult to effectively remove thiophene macromolecular sulfides in liquid methane. Traditional desulfurizers cannot be used in gaseous methane, and their ability to remove macromolecular sulfides such as tetrahydrothiophene and benzothiophene is limited.
Graphene-ionic liquid composite materials are used as sulfur adsorbents. By designing π-π stacking effects and ionic liquid structures, the adsorption capacity of thiophene aromatic hydrocarbon sulfides is improved. The preparation method includes the reaction of graphene oxide and cationic bromide salts and ions. The combination of liquids creates an efficient sulfur adsorbent.
It achieves efficient adsorption of thiophene aromatic hydrocarbon sulfides in methane, and the adsorption efficiency is significantly higher than that of traditional materials, solving the problem of difficulty in removing macromolecular sulfides in methane propellant.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of graphene composite materials, and particularly relates to a preparation method and application of a graphene-ionic liquid composite sulfur adsorbent. Background Art
[0002] Liquid oxygen / methane engines have outstanding advantages such as high specific impulse, low cost, non-toxic and pollution-free, low carbon deposition, and reusability, and are a hot topic of research for major aerospace powers. The liquid oxygen / methane propellant combination has been selected by NASA as the main development direction of future chemical space propellants and is recognized as an ideal power choice for future spacecraft. In May 2019, my country's first 80-ton liquid oxygen-methane engine "Tianque" (TQ-12) was successfully tested, becoming the world's third high-thrust liquid oxygen-methane rocket engine to complete full system test and assessment.
[0003] Liquid methane propellant, as the power source for liquid oxygen / methane engines, is mainly obtained through natural purification and then liquefaction. Although natural gas is purified during the liquefaction process, due to process limitations, there is still a certain amount of sulfur compounds in liquid methane propellant, mainly including mercaptans, sulfides, thiophenes, etc. Sulfides are corrosive, and their content exceeds the standard can corrode the engine fuel channel. In severe cases, coking will occur, causing channel blockage. Therefore, the sulfur content in the propellant-grade methane standards of various countries has been detailed. However, it is difficult to remove thiophene aromatic sulfides only through traditional purification treatments such as distillation. Developing a desulfurization adsorbent with high selectivity for sulfides in liquid methane is the technical key to obtaining methane with ultra-low sulfur content.
[0004] The currently disclosed desulfurizers are mainly used in the field of desulfurization of oils such as gasoline and diesel. The currently disclosed graphene-type desulfurizers (CN 104525063 A, CN 113755205 A) are all based on the principle of oxidative desulfurization. Generally, the method of use is to mix the desulfurizer and fuel oil evenly, then add an oxidative desorbent, let it stand for a period of reaction to separate the catalyst from the fuel, and take the fuel layer to separate the catalyst from the fuel. Methane is gaseous at room temperature, and its desulfurization method is generally dry desulfurization, that is, the sulfide in the gas is removed. The above-mentioned adsorbent cannot be used for desulfurization in methane gas; and traditional desulfurization technology and desulfurization materials have a strong removal ability for hydrogen sulfide gas, but due to the presence of macromolecular sulfides such as tetrahydrothiophene, benzothiophene, dibenzothiophene, and 4,6-dimethyldibenzothiophene in liquid methane, it is difficult for traditional desulfurization technology to remove them.
[0005] Graphene is a new type of carbon nanomaterial with a conjugated system, large specific surface area and excellent chemical stability. Graphene can produce a strong π-π stacking effect with organic molecules with a benzene ring structure, making it a potential high-efficiency material for adsorbing thiophene aromatic sulfides. However, due to its ultra-light weight and easy aggregation, graphene cannot be used directly as an adsorption material.
[0006] Ionic liquids have a wide liquid temperature range, can dissolve a variety of organic and inorganic substances, have low vapor pressure and good stability, and are widely used in organic synthesis, extraction separation, electrochemistry, and nanomaterial preparation. Selectivity for the target compound can be achieved through ionic liquid structural design, but there are few reports on liquid methane desulfurization adsorbents. Summary of the invention
[0007] In view of the current technical problems, the present invention provides a preparation method and application of a graphene-ionic liquid composite sulfur adsorbent. The adsorbent has a strong adsorption capacity for sulfides and can adsorb thiophene aromatic sulfides in liquid methane, thereby solving the purification problem of liquid methane propellant.
[0008] The technical solution of the present invention is as follows:
[0009] A method for preparing a graphene-ionic liquid composite sulfur adsorbent, the specific steps are as follows:
[0010] (1) adding a cationic salt and a brominated alkane, stirring and reacting at 50 to 70° C. for 16 to 24 hours, filtering, and washing with ethanol to obtain a cationic bromide salt;
[0011] (2) ultrasonically dispersing graphene oxide in an acetone solvent, adding cationic bromide and NaBF4, passing nitrogen protection, stirring at 50-70° C. for 16-24 h, filtering, washing with dichloromethane, and drying to obtain a product;
[0012] (3) dispersing the product in water, adding neutral salt, stirring evenly, adding hydrazine hydrate solution and ammonia solution, reacting at 80-120° C. for 6-12 hours, centrifuging, washing with water, and freeze-drying to obtain a graphene-ionic liquid composite material.
[0013] The preparation method of graphene oxide is as follows: in an ice-water bath, concentrated sulfuric acid, potassium permanganate and sodium nitrate are added in sequence, and after being mixed evenly, expandable graphite powder is slowly added, and the mixture is allowed to stand in an ice bath environment for 24 to 36 hours; then the temperature is raised to 30 to 40°C, stirred for 25 to 35 minutes, deionized water is slowly added, and the system is heated to 93 to 103°C, and stirring is continued for 15 minutes, and the product is allowed to stand and precipitate, the upper clear liquid is poured out, hydrogen peroxide is added, and the precipitate is washed with hydrochloric acid aqueous solution and deionized water in sequence until the pH is neutral, and then dried. The dried graphite oxide powder is ultrasonically dispersed in distilled water, centrifuged to obtain a graphene oxide sol, and dried to obtain graphene oxide.
[0014] Further preferably, in the system for preparing graphene oxide, the concentration of potassium permanganate is 0.03-0.05 mg / mL, the concentration of sodium nitrate is 0.02-0.04 mg / mL, and the concentration of expandable graphite powder is 0.02-0.04 mg / mL; the volume ratio of concentrated sulfuric acid, deionized water, and hydrogen peroxide is 90-150:180-250:30-50; in step (1), the volume fraction of the hydrochloric acid aqueous solution is 5%-10%, and the volume concentration of hydrogen peroxide is 20%-30%. Further preferably, the volume fraction of the hydrochloric acid aqueous solution is 5%, and the volume concentration of hydrogen peroxide is 30%.
[0015] Preferably, in step (1), the molar ratio of the cationic salt to the brominated alkane is 1:1 to 1:3.
[0016] Preferably, the cation in the cationic salt is one of imidazolium salt cations, quaternary ammonium salt cations, quaternary phosphonium salt cations and pyridinium salt cations.
[0017] Preferably, the brominated alkane is one of n-propane bromide, isopropane bromide, sec-butyl bromide, n-butyl bromide, n-pentane bromide and n-hexane bromide.
[0018] Preferably, in step (2), the mass ratio of graphene oxide to cationic salt is 1:10 to 1:50, the molar ratio of cationic salt to NaBF4 is 1:1 to 1:3, and the concentration of graphene oxide dispersed in acetone is 2 to 10 mg / mL.
[0019] Preferably, in step (3), the neutral salt is one of sodium chloride and potassium chloride, and the concentration is 0.1 to 0.5 mol / L.
[0020] Preferably, in step (3), the product is dispersed in water at a concentration of 10 to 50 mg / mL, and the volume ratio of water: hydrazine hydrate solution: ammonia water is 5:1:1 to 8:1:2. Further preferably, the mass concentration of the hydrazine hydrate solution is 80%, and the mass concentration of the ammonia water is 25%.
[0021] Application of a graphene-ionic liquid composite sulfur adsorbent in methane desulfurization.
[0022] The graphene-ionic liquid composite sulfur adsorbent prepared by the present invention has an excellent removal effect on macromolecular sulfides such as thiophenes. The inventors have found through exploration that graphene can produce a strong π-π stacking effect with macromolecules such as thiophene having a benzene ring structure, and has extremely strong adsorption capacity; secondly, through the design of the ionic liquid structure, it has a certain selectivity for macromolecular sulfides such as thiophene, thereby improving the desulfurization capacity.
[0023] A novel graphene-ionic liquid composite sulfur adsorbent prepared by the present invention can adsorb thiophene aromatic sulfides in methane, solve the purification problem of methane propellant, and for the first time solve the difficult problem of removing large molecular sulfides such as thiophene in methane. Compared with traditional adsorption materials, this material has high adsorption efficiency and simple preparation method. DETAILED DESCRIPTION
[0024] The present invention is not limited by the following embodiments. The following embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may be subject to various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
[0025] Example 1
[0026] A method for preparing graphene oxide:
[0027] Under 0°C ice-water bath conditions, 90mL of concentrated sulfuric acid (mass fraction of 98%), 12g of potassium permanganate, and 2g of sodium nitrate were added to a 500mL round-bottom flask in sequence, and after mixing evenly, 2g of expandable graphite powder (particle size <30μm) was slowly added, and the mixture was allowed to stand in an ice bath environment at 0°C for 24h, and then the temperature was raised to 35°C, stirred for 30min, and 180mL of deionized water was slowly added. When the system was heated to (98±5)°C, stirring was continued for 15min, and the product was allowed to stand and precipitate, the supernatant was poured out, 50mL of 30% hydrogen peroxide was added, and the precipitate was washed with a 5% hydrochloric acid aqueous solution and deionized water in sequence until the pH was neutral, and the product was dried at 60°C, the dried product was ultrasonically dispersed in 20mL of distilled water, and centrifuged to obtain a graphene oxide sol, and the product was dried at 60°C to obtain graphene oxide.
[0028] The graphene oxides in Examples 2-3 are all selected from the graphene oxide prepared in Example 1.
[0029] Example 2
[0030] A method for preparing a graphene-ionic liquid composite sulfur adsorbent:
[0031] (1) Preparation of 1-n-propyl-3-methylimidazolium bromide: 0.1 mol N-methylimidazole and 0.1 mol n-propane bromide were added to a 500 mL round-bottom flask, stirred at 60° C. for 16 h, filtered, and washed with ethanol to obtain 1-n-propyl-3-methylimidazolium bromide;
[0032] (2) 1 g of graphene oxide was ultrasonically dispersed in 150 mL of acetone solvent, and 0.1 mol of 1-n-propyl-3-methylimidazolium bromide and 0.1 mol of NaBF4 were added respectively. The mixture was protected by nitrogen and stirred at 60°C for 16 h. The mixture was filtered, washed with 50 mL of dichloromethane, and dried at 60°C to obtain the product. The product was redispersed in 100 mL of water, 1.17 g of sodium chloride was added, and the mixture was stirred evenly. 20 mL of hydrazine hydrate solution (mass concentration of 80%) and 20 mL of ammonia solution (mass concentration of 25%) were added respectively. The mixture was heated at 80°C for 6 h, centrifuged, washed with water, and frozen (minus 20°C) and dried for 24 h to obtain graphene-ionic liquid composite material A.
[0033] The tetrahydrothiophene content in methane was detected by gas chromatography flame photometric detector (FPD) and was 500ug / g. 8g of composite material A was loaded into a stainless steel column (outer diameter 6.35mm, length 89mm), and the stainless steel column was connected to the gas cylinder through a pressure reducing valve. The tetrahydrothiophene content in methane after adsorption was measured to be 36ug / g, and the adsorption efficiency was 93%.
[0034] Example 3
[0035] A method for preparing a graphene-ionic liquid composite sulfur adsorbent:
[0036] (1) Preparation of N-butylpyridinium bromide: 0.1 mol of pyridine and 0.1 mol of n-butyl bromide were added to a 500 mL round-bottom flask, stirred at 60° C. for 16 h, filtered, and washed with ethanol to obtain a white solid crude product of N-butylpyridinium bromide;
[0037] (2) 1 g of graphene oxide was ultrasonically dispersed in 150 mL of acetone solvent, and 0.1 mol of N-butylpyridinium bromide and 0.1 mol of NaBF4 were added respectively. The mixture was protected by nitrogen and stirred at 70°C for 20 h. The mixture was filtered and washed with 50 mL of dichloromethane. The product was dried at 60°C. The product was redispersed in 100 mL of water, and 0.5 mol / L of sodium chloride was added. The mixture was stirred evenly. 20 mL of hydrazine hydrate solution (mass concentration of 80%) and 20 mL of ammonia solution (mass concentration of 25%) were added respectively. The mixture was heated at 100°C for 10 h, centrifuged, washed with water, and freeze-dried (minus 20°C) for 24 h to obtain graphene-ionic liquid composite material B.
[0038] The content of 4,6-dimethyldibenzothiophene in methane was detected by gas chromatography flame photometric detector (FPD), which was 450ug / g. 8g of composite material B was loaded into a stainless steel column (outer diameter 6.35mm, length 89mm), and the stainless steel column was connected to the gas cylinder through a pressure reducing valve. The content of 4,6-dimethyldibenzothiophene in methane after adsorption was measured to be 10ug / g, and the adsorption efficiency was 98%.
[0039] Comparative Example 1
[0040] Activated carbon is a commonly used methane desulfurization agent, and commercially available activated carbon is used as the desulfurization agent.
[0041] The content of 4,6-dimethyldibenzothiophene in methane was detected by gas chromatography flame photometric detector (FPD), which was 450ug / g. 8g of activated carbon was loaded into a stainless steel column (outer diameter 6.35mm, length 89mm), and the stainless steel column was connected to the gas cylinder through a pressure reducing valve. The content of 4,6-dimethyldibenzothiophene in methane after adsorption was measured to be 135ug / g, and the adsorption efficiency was 70%.
[0042] Through the above comparison, it can be found that the adsorption efficiency of the adsorption desulfurizer prepared in Examples 2-3 is above 93%, which is significantly higher than the adsorption efficiency of the activated carbon in Comparative Example 1. A novel graphene-ionic liquid composite sulfur adsorbent prepared by the present invention can adsorb thiophene aromatic sulfides in methane and solve the purification problem of methane propellant. Compared with traditional adsorption materials, the material has high adsorption efficiency and simple preparation method.
Claims
1. A method for preparing a graphene-ionic liquid composite sulfur adsorbent, characterized in that: The specific steps are as follows: (1) Add cationic salt and bromoalkane, stir and react at 50-70°C for 16-24 hours, filter and wash with ethanol to obtain cationic bromide salt; The molar ratio of the cationic salt to the bromoalkane is 1:1 to 1:3, the cation in the cationic salt is one of imidazolium salt cations, quaternary ammonium salt cations, quaternary phosphonium salt cations and pyridinium salt cations, and the bromoalkane is one of n-propane bromide, isopropane bromide, sec-butyl bromide, n-butyl bromide, n-pentane bromide and n-hexane bromide; (2) Ultrasonic dispersion of graphene oxide in acetone solvent, then adding cationic bromide and NaBF4, passing nitrogen protection, stirring at 50-70°C for 16-24h, filtering, washing with dichloromethane, and drying to obtain the product; The mass ratio of graphene oxide to cationic salt is 1:10-1:50, the molar ratio of cationic salt to NaBF4 is 1:1-1:3, and the concentration of graphene oxide dispersed in acetone is 2-10 mg / mL; (3) Dispersing the product in water, adding neutral salt, stirring evenly, adding hydrazine hydrate solution and ammonia solution, reacting at 80-120° C. for 6-12 hours, centrifuging, washing with water, and freeze-drying to obtain a graphene-ionic liquid composite material; wherein the neutral salt is one of sodium chloride and potassium chloride, and the concentration is 0.1-0.5 mol / L.
2. The method for preparing a graphene-ionic liquid composite sulfur adsorbent according to claim 1, characterized in that: The preparation method of the graphene oxide is as follows: in an ice-water bath, concentrated sulfuric acid, potassium permanganate and sodium nitrate are added in sequence, mixed evenly, expandable graphite powder is slowly added, and the mixture is allowed to stand in an ice bath environment for 24 to 36 hours; then the temperature is raised to 30 to 40° C., stirred for 25 to 35 minutes, deionized water is slowly added, and the system is heated to 93 to 103° C., stirred for 15 minutes, and the product is allowed to stand and precipitate, the upper clear liquid is poured out, hydrogen peroxide is added, and the precipitate is washed with hydrochloric acid aqueous solution and deionized water in sequence until the pH is neutral, dried, and then ultrasonically dispersed in distilled water, centrifuged to obtain a graphene oxide sol, and dried to obtain graphene oxide.
3. The method for preparing a graphene-ionic liquid composite sulfur adsorbent according to claim 2, characterized in that: In the system for preparing graphene oxide, the concentration of potassium permanganate is 0.03-0.05 mg / mL, the concentration of sodium nitrate is 0.02-0.04 mg / mL, and the concentration of expandable graphite powder is 0.02-0.04 mg / mL; the volume ratio of concentrated sulfuric acid, deionized water, and hydrogen peroxide is 90-150:180-250:30-50.
4. The method for preparing a graphene-ionic liquid composite sulfur adsorbent according to claim 1, characterized in that: In step (3), the product is dispersed in water at a concentration of 10 to 50 mg / mL, and the volume ratio of water: hydrazine hydrate solution: ammonia water is 5:1:1 to 8:1:
2.
5. Use of the graphene-ionic liquid composite sulfur adsorbent prepared by the method according to any one of claims 1 to 4 in methane desulfurization.
Citation Information
Patent Citations
Graphene aerogel loaded with polyionic liquid-NaBH4-NiCl2 system and preparation method thereof
CN104525063A
Fuel oil desulfurization purification method
CN113755205A
Preparation method of graphene-based conductive ink filler
CN107057409A
Amino ionic liquid modified graphene oxide for adsorbing sulfur dioxide and preparation method of amino ionic liquid modified graphene oxide
CN107824162A
Method for purifying sulfides in liquid methane propellant
CN113277925A