A transition metal element supported cerium-based catalyst and its preparation method and use
By loading monodisperse sub-nanometer atomic clusters of transition metal elements onto the surface of cerium dioxide, the problem of insufficient catalyst activity was solved, achieving efficient catalytic oxidation of carbon monoxide and reducing costs.
Patent Information
- Application Number
- CN202310076561.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-01-16
AI Technical Summary
The dispersion of existing transition metal elements on the surface of cerium oxide support is difficult to control, resulting in insufficient number of catalyst active sites or passivation of transition metal sites, which affects the efficiency of catalytic oxidation of carbon monoxide.
By designing the loading method, transition metal elements are made to exist as monodisperse sub-nanometer atomic clusters on the surface of cerium dioxide, anchored on oxygen vacancies, forming a porous material, thereby improving the activity and stability of the catalyst.
The catalyst achieves high efficiency in catalytic oxidation of carbon monoxide, is low in cost, and is comparable to precious metal catalysts, making it suitable for emission control of high-concentration CO waste gas.
Smart Images

Figure CN115970679B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a highly dispersed cerium-based catalyst of transition metal elements for efficiently catalyzing the oxidation of carbon monoxide (CO), a preparation method and application thereof, and belongs to the field of catalysts. Background Art
[0002] Carbon monoxide (CO) is a common air pollutant. It not only has high biological toxicity at low concentrations, but also can participate in atmospheric photochemical reactions to form secondary pollution such as photochemical smog, reduce atmospheric oxidation and prolong the atmospheric residence time of greenhouse gases. CO is mainly produced by incomplete combustion of fossil fuels and is widely emitted in industries such as steel, coking, industrial boilers, coal-fired power generation, and heating boilers. Among them, the concentration of CO in the flue gas of the steel and coking industries usually reaches 0.5-1 vol%, and it needs to be purified and removed before it can meet the emission standards.
[0003] The catalytic oxidation method has high efficiency and low cost, and is an important method to achieve CO emission reduction. While reducing the outlet CO emission concentration, it can also use oxidation heat to increase the flue gas temperature, which is beneficial to the subsequent treatment of industrial flue gas. At present, most catalytic oxidation CO technologies use precious metal catalysts, which have excellent catalytic performance, but are expensive and easily deactivated due to precious metal loss, sintering, poisoning, etc. Cerium-based catalysts have excellent redox properties, high oxygen storage capacity and oxygen mobility, and are relatively cheap and abundant in reserves. Moreover, transition metals are good active sites. The use of transition metal elements such as Cu, Mn, and Co as active ingredients is very important for the development of cheap, efficient, and stable CO catalysts. Therefore, considering the cost advantages and performance prospects of non-precious metal elements, transition metal element-supported cerium-based catalysts have good prospects for replacing supported precious metal catalysts to achieve industrial applications.
[0004] However, the dispersion of transition metal elements on the surface of cerium oxide carriers is difficult to control. For the commonly used loading methods, such as US9815044B2, the low dispersion of the loaded elements will make it difficult to increase the number of active sites at the contact surface, resulting in insufficient activity; the single atomic dispersion of the loaded elements, such as CN112044434A, will easily passivate the transition metal sites, which is also not conducive to improving activity. Therefore, the technical challenge currently faced is to increase the content of highly active reaction sites and improve the performance of catalysts for catalytic oxidation of CO by regulating the high dispersion of loaded transition metal elements on the surface of cerium oxide in the form of sub-nanometer atomic clusters. Summary of the invention
[0005] Problem that the invention aims to solve
[0006] In order to overcome the above-mentioned shortcomings of the prior art, it is necessary to provide a catalyst that can improve the catalytic activity while ensuring the stability of the catalyst structure.
[0007] Therefore, the purpose of the present invention is to provide a highly efficient catalytic oxidation of CO, a structurally stable transition metal element highly dispersed supported cerium-based catalyst, and a preparation method and use thereof.
[0008] Solutions for solving problems
[0009] In the present invention, by designing the loading method, the catalytic activity can be improved while ensuring the stability of the catalyst structure. The transition metal elements loaded by the catalyst of the present invention are highly dispersed sub-nanometer atomic clusters, have good atomic utilization and excellent electronic structure, and show more excellent catalytic performance.
[0010] [1] The present invention provides a transition metal element supported cerium-based catalyst, characterized in that the catalyst is a porous material composed of crystal particles formed by cerium dioxide as a carrier supporting a transition metal element, and the catalyst is represented by the formula M / CeO2, wherein M is a transition metal element,
[0011] The transition metal element is in the form of monodispersed sub-nanometer atomic clusters with a size of 1 to 5 nm on the surface of the cerium dioxide.
[0012] [2] The catalyst according to [1] above, wherein the transition metal element is anchored to oxygen vacancies on the surface of ceria as a support.
[0013] [3] The catalyst according to [1] or [2] above, wherein the molar ratio of the transition metal element to the cerium dioxide is 1:5 to 1:200, preferably 1:20 to 1:100.
[0014] [4] The catalyst according to any one of [1] to [3] above, wherein the diameter of the crystallites is 5 to 100 nm, preferably 5 to 20 nm; the pore size of the porous material is 5 to 100 nm, preferably 5 to 20 nm; the BET surface area of the porous material is 5 to 150 m 2 ·g -1 , preferably 50~150m 2 ·g -1 .
[0015] [5] The catalyst according to any one of [1] to [4] above, wherein the transition metal element is selected from one or more of manganese, iron, cobalt, nickel and copper.
[0016] [6] The present invention also provides a method for preparing a transition metal element supported cerium-based catalyst, characterized in that the preparation method comprises the following steps:
[0017] Step 1: dispersing the cerium dioxide carrier into the first solvent by ultrasonication to obtain a suspension;
[0018] Step 2: dissolving a transition metal element precursor in a second solvent to obtain a clear solution;
[0019] Step 3: adding the clarified solution obtained in step 2 to the suspension obtained in step 1 and stirring to obtain a mixed solution;
[0020] Step 4: transferring the mixed solution obtained in step 3 to a hydrothermal reaction kettle for hydrothermal reaction;
[0021] Step 5: Separate, wash, dry and calcine the solid obtained by the hydrothermal reaction in step 4 to obtain a transition metal element-supported cerium-based catalyst in which the transition metal element is supported on cerium dioxide as a carrier.
[0022] [7] According to the preparation method described in [6] above, in the suspension in step 1, the mass concentration of the cerium dioxide carrier is 5-200 g / L, preferably 20-100 g / L; the molar ratio of the transition metal element precursor used in step 2 to the cerium dioxide carrier used in step 1 is 1:5-1:200, preferably 1:20-1:100; in the clear solution, the molar concentration of the transition metal element precursor is 0.001-0.04 mol / L, preferably 0.003-0.01 mol / L.
[0023] [8] The preparation method according to [6] or [7] above, wherein the transition metal element precursor is selected from a mixture of one or more of manganese nitrate, manganese chloride, manganese fluoride, manganese sulfate, manganese acetate, manganese oxalate, manganese bromide, ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferric fluoride, ferrous fluoride, ferric sulfate, ferrous sulfate, ferric acetate, ferrous acetate, ferrous oxalate, ferrous oxalate, ferric bromide, ferrous bromide, cobalt nitrate, cobalt chloride, cobalt fluoride, cobalt sulfate, cobalt acetate, cobalt oxalate, cobalt bromide, nickel nitrate, nickel chloride, nickel fluoride, nickel sulfate, nickel acetate, nickel oxalate, nickel bromide, copper nitrate, copper chloride, copper fluoride, copper sulfate, copper acetate, copper oxalate, and copper bromide; the first solvent and the second solvent are selected from a mixture of one or more of water, ethanol, methanol, ethylene glycol, and acetone; and the first solvent and the second solvent are the same or different.
[0024] [9] The preparation method according to any one of [6] to [8] above, wherein in step 1, the ultrasonic dispersion time is 1 to 200 min, preferably 20 to 100 min; in step 3, the stirring time is 0.5 to 12 h, preferably 1 to 8 h; in step 4, the hydrothermal temperature is 50 to 150°C, preferably 80 to 120°C, and the hydrothermal time is 0.5 to 36 h, preferably 6 to 24 h; in step 5, the calcination is carried out under the condition of an oxygen content of 1 to 100 vol%, the calcination temperature is 200 to 800°C, preferably 400 to 600°C, and the calcination time is 0.5 to 12 h, preferably 4 to 8 h.
[0025]
[10] The present invention further provides a use of the catalyst according to any one of [1] to [5] above or the catalyst obtained by the preparation method according to any one of [6] to [9] above for removing CO from exhaust gas.
[0026] Effects of the Invention
[0027] The technical solution of the present invention can have the following beneficial effects:
[0028] (1) The transition metal elements loaded in the catalyst disclosed in the present invention are in the form of highly dispersed sub-nanometer atomic clusters on the surface of the ceria carrier, have good atomic utilization and an electronic structure that is conducive to CO adsorption and reaction, have excellent catalytic activity, are similar to existing commercial precious metal catalysts, and achieve significant cost reduction.
[0029] (2) The preparation method of the present invention is simple, low-cost, and can be produced on a large scale, thus having commercial prospects.
[0030] (3) The catalyst of the present invention can be used at 100 to 500°C, has a wide operating temperature range, and a low activation temperature, and can be widely used in the emission control of high-concentration CO in waste gases such as boiler flue gas, blast furnace flue gas, and coking flue gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The graph showing the relationship between the conversion rate of catalytic oxidation of CO and temperature of the catalysts of Example 1, Example 2 and Comparative Example 1 of the present invention.
[0032] Figure 2 Shown are a transmission electron microscope image (a) and a spherical aberration corrected scanning transmission electron microscope image (b) of the catalyst of Example 1 of the present invention, an X-ray diffraction spectrum (c) and an X-ray absorption fine structure spectrum (d) of the catalyst of Example 1 of the present invention, and Raman spectra (e) and (f) of the catalysts of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0033] In order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.
[0034] Unless otherwise stated, the units used in the present invention are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0035] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0036] Unless otherwise required in this application, throughout the specification and the claims that follow, the word "comprising" should be interpreted in its open, inclusive sense, ie, "including, but not limited to."
[0037] In this specification, unless otherwise specified, the word "multiple" in "multiple", "multiple", "plurality", etc. means a numerical value of 2 or more.
[0038] In the present specification, the term “substantially”, “substantially” or “essentially” means that the error is less than 5%, less than 3% or less than 1% compared with the relevant perfect standard or theoretical standard.
[0039] In this specification, the word "may" includes both performing a certain process and not performing a certain process.
[0040] In the present specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes cases where the event occurs and cases where it does not occur.
[0041] In this specification, if "room temperature" or "normal temperature" appears, the temperature may generally be 10-40°C.
[0042] In this specification, "monodisperse" has the common meaning in the art, and in the present invention means that the atomic clusters of the transition metal element are substantially uniform in size and are uniformly dispersed on the cerium dioxide as a carrier.
[0043] <First aspect>
[0044] The first aspect of the present invention provides a transition metal element supported cerium-based catalyst, wherein the catalyst is a porous material composed of crystal grains formed by cerium dioxide as a carrier and a transition metal element, wherein the transition metal element is in the form of a monodispersed sub-nanometer atomic cluster with a size of 1 to 5 nm on the surface of the cerium dioxide. The catalyst crystal grain size is uniform, and the diameter of a single crystal grain is 5 to 100 nm. The crystal grains are randomly stacked to form channels with a pore size of 5 to 100 nm. The BET surface area of the catalyst of the present invention is 5 to 150 m 2 ·g -1 , preferably 50~150m 2 ·g -1 , more preferably 100 to 150 m 2 ·g -1 .
[0045] The uniform grain size can ensure the homogeneity of the catalyst and improve the performance of further coating and utilization. The porous structure is conducive to the mass transfer and adsorption of CO. If the diameter of a single crystal grain is too small, it is difficult to synthesize and easier to sinter. If the diameter is too large, the specific surface area of the catalyst is small, which is not conducive to increasing the concentration of reaction sites. Preferably, the diameter of a single crystal grain is 5 to 80 nm, more preferably 5 to 50 nm, and even more preferably 5 to 20 nm. If the pore size of the channel formed by the accumulation is too small, it is not conducive to the diffusion of the reactants. If the pore size is too large, the specific surface area is small, which is not conducive to increasing the concentration of reaction sites. Preferably, the pore size is 5 to 80 nm, more preferably 5 to 50 nm, and even more preferably 5 to 20 nm.
[0046] In the present invention, the transition metal element supported cerium-based catalyst can be represented by the formula M / CeO2, wherein M is a transition metal element. Specifically, the transition metal element can be selected from one or more of manganese, iron, cobalt, nickel, copper, etc. The loading of transition metal elements can provide more effective reactant adsorption sites, induce the improvement of the redox performance and oxygen storage and release capacity of the cerium oxide support, and regulate the dominant reaction path.
[0047] In the catalyst of the present invention, the transition metal elements are in the form of monodisperse sub-nano atomic clusters with a size of 1 to 5 nm on the surface of cerium dioxide, which are evenly dispersed, do not agglomerate, and are anchored on the oxygen vacancies on the surface of the carrier CeO2. Specifically, the size of the sub-nano atomic clusters can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, etc. Uniform and highly dispersed loaded atomic clusters are conducive to increasing the number of active sites at the contact surface, and agglomeration will weaken the above effect; anchoring on oxygen vacancies increases the intensity of the interaction between the surface active components and the carrier, optimizes the electronic structure of the reaction active sites, and is conducive to improving the reaction activity.
[0048] In the catalyst of the present invention, the molar ratio of the transition metal element to the cerium dioxide is 1:5 to 1:200, preferably 1:20 to 1:100, and more preferably 1:25 to 1:50. The mass ratio of the transition metal element to the cerium oxide carrier can regulate the loading amount of the catalyst. Too low loading amount will result in a small number of active sites and limited improvement in catalytic performance. Too high loading amount will lead to agglomeration of the transition metal loading, which is not conducive to the formation of interfacial active sites.
[0049] The transition metal elements loaded in the catalyst of the present invention are in the form of highly dispersed sub-nanometer atomic clusters, and have excellent catalytic activity similar to that of existing commercial noble metal catalysts, while achieving significant cost reduction.
[0050] <Second Aspect>
[0051] The second aspect of the present invention provides a method for preparing the catalyst of the present invention, which comprises the following steps:
[0052] Step 1: dispersing the cerium dioxide carrier into the first solvent by ultrasonication to obtain a suspension;
[0053] Step 2: dissolving a transition metal element precursor in a second solvent to obtain a clear solution;
[0054] Step 3: adding the clarified solution obtained in step 2 to the suspension obtained in step 1 and stirring to obtain a mixed solution;
[0055] Step 4: transferring the mixed solution obtained in step 3 to a hydrothermal reaction kettle for hydrothermal reaction;
[0056] Step 5: Separate, wash, dry and calcine the solid obtained by the hydrothermal reaction in step 4 to obtain a transition metal element-supported cerium-based catalyst in which the transition metal element is supported on cerium dioxide as a carrier.
[0057] Each step is described in detail below.
[0058] Step 1
[0059] In the step 1, the mass concentration of the carrier in the suspension is 5 to 200 g / L, preferably 20 to 100 g / L, more preferably 20 to 50 g / L. The ultrasonic dispersion time is 1 to 200 min, preferably 20 to 100 min, more preferably 20 to 60 min.
[0060] The above steps to obtain the cerium oxide carrier suspension can enable the carrier to achieve better dispersion before loading, which is helpful for further sufficient contact between the loaded transition element precursor and the carrier, so as to obtain a uniformly loaded catalyst.
[0061] In the present invention, there is no particular limitation on the morphology of the ceria used as a carrier. For example, the ceria carrier may include a mixture of one or more cerium oxide nanocrystals and microcrystals of different morphologies such as rod-shaped ceria, cubic ceria, octahedral ceria, spherical ceria, flake ceria, spindle-shaped ceria, bouquet-shaped ceria, and irregular-shaped ceria.
[0062] The first solvent may be a mixture of one or more of water, ethanol, methanol, ethylene glycol and acetone.
[0063] The specific operation includes: weighing a certain amount of cerium oxide carrier, measuring a certain amount of solvent, adding the weighed cerium oxide carrier into the solvent while vigorously stirring the solvent, and placing the suspension into an ultrasonic cleaner for further dispersion to obtain a carrier suspension.
[0064] Step 2
[0065] In step 2, the molar ratio of the transition metal element precursor used to the cerium oxide support used in step 1 is 1:5-1:200, preferably 1:20-1:100. The molar concentration of the transition metal element precursor solution is 0.001-0.04 mol / L, preferably 0.003-0.01 mol / L.
[0066] The mass ratio of transition metal element precursor to cerium oxide carrier can regulate the loading amount of the catalyst. Too low loading amount will lead to a small number of active sites and limited improvement in catalytic performance. Too high loading amount will cause transition metal load agglomeration, which is not conducive to the formation of interfacial active sites. The concentration of transition metal element solution is required to reduce solvent waste while ensuring that the precursor can be completely dissolved.
[0067] In the present invention, the transition metal element precursor can be a mixture of one or more of manganese nitrate, manganese chloride, manganese fluoride, manganese sulfate, manganese acetate, manganese oxalate, manganese bromide, ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferrous fluoride, ferrous fluoride, ferric sulfate, ferrous sulfate, ferrous acetate, ferrous acetate, ferrous oxalate, ferrous oxalate, ferrous bromide, ferrous bromide, cobalt nitrate, cobalt chloride, cobalt fluoride, cobalt sulfate, cobalt acetate, cobalt oxalate, cobalt bromide, nickel nitrate, nickel chloride, nickel fluoride, nickel sulfate, nickel acetate, nickel oxalate, nickel bromide, copper nitrate, copper chloride, copper fluoride, copper sulfate, copper acetate, copper oxalate, and copper bromide.
[0068] In the present invention, the second solvent may be a mixture of one or more of water, ethanol, methanol, ethylene glycol, and acetone. Furthermore, the second solvent may be the same as or different from the first solvent.
[0069] The specific operation includes: weighing a certain amount of transition metal element precursor, measuring a certain amount of solvent, adding the weighed precursor into the solvent, stirring and dissolving to obtain a precursor solution.
[0070] Step 3
[0071] In the step 3, the stirring time is 0.5 to 12 hours, preferably 1 to 8 hours.
[0072] Within the above stirring time range, the transition element precursor can be fully contacted with the cerium oxide carrier, so as to obtain a uniformly loaded catalyst later and ensure the high dispersion of the transition element loading. Too short a stirring time will lead to insufficient mixing.
[0073] The specific operation includes: adding the precursor solution into the carrier suspension under vigorous stirring, and continuing to stir vigorously.
[0074] Step 4
[0075] In step 4, the hydrothermal time is 0.5 to 36 hours, preferably 6 to 24 hours, and the hydrothermal temperature is 50 to 150° C., preferably 80 to 120° C.
[0076] Within the above-mentioned time and temperature range, the transition elements and the carrier can fully react to form a strong interaction, so that the transition metal elements can be stably anchored on the oxygen vacancies of the cerium oxide carrier in the form of sub-nanometer atomic clusters. If the time is too short or the temperature is too low, the transition elements cannot be stably loaded on the carrier surface and the dispersion is insufficient. If the time is too long or the temperature is too high, the structural morphology of the cerium oxide carrier may be destroyed.
[0077] The specific operation includes: transferring the mixture obtained in step 3 to a hydrothermal autoclave lined with polytetrafluoroethylene, placing the hydrothermal autoclave in a pre-heated oven, and taking it out and cooling it after the reaction is completed.
[0078] Step 5
[0079] In step five, the calcination is carried out under the condition of oxygen content of 1 to 100%, the calcination time is 0.5 to 12 hours, preferably 4 to 8 hours, and the calcination temperature is 200 to 800° C., preferably 400 to 600° C.
[0080] Within the above calcination time and temperature range, the catalyst can be activated and stabilized. If the time is too short or the temperature is too low, the calcination effect cannot be achieved. If the temperature is too high or the time is too long, the catalyst may sinter and become inactivated.
[0081] The catalyst preparation method of the present invention is simple, low in cost and has commercial prospects.
[0082] <Third Aspect>
[0083] The present invention also provides a use of the catalyst of the present invention for removing CO from exhaust gas.
[0084] The catalyst of the present invention is used at a temperature of 100 to 500° C., and the waste gas includes waste gas containing relatively high concentration of CO discharged from industrial processes such as boiler flue gas, blast furnace flue gas, and coking flue gas.
[0085] Example
[0086] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0087] Example 1
[0088] Copper element is selected as the transition element load, and rod-shaped cerium oxide nanoparticles synthesized by hydrothermal method are used as the carrier. The preparation steps of copper element highly dispersed loaded rod-shaped cerium-based (Cu / CeO2) catalyst are as follows:
[0089] Step 1: Weigh 1.000g of cerium oxide carrier, measure 40mL of deionized water, add CeO2 into the deionized water and stir vigorously, put the obtained suspension into an ultrasonic cleaner for 30 minutes to obtain a well-dispersed carrier suspension;
[0090] Step 2: Weigh 0.036 g of copper acetate hexahydrate, measure 40 mL of deionized water, dissolve the weighed copper acetate hexahydrate in the deionized water, and stir until completely dissolved to obtain a clear solution;
[0091] Step 3: Add the clarified solution obtained in step 2 to the suspension obtained in step 1, and stir vigorously at a speed of 450 r / min for 2 h to obtain a mixed solution;
[0092] Step 4: Transfer the mixed solution obtained in step 3 to a polytetrafluoroethylene reactor with a capacity of 100 ml, tighten the stainless steel hydrothermal reactor, and perform a hydrothermal reaction for 12 hours in a constant temperature oven preheated to 100°C;
[0093] Step 5: Filter and separate the solid treated in step 4, wash it with deionized water and ethanol in turn, dry it at 60°C overnight, and calcine it at 400°C for 4 hours in air (oxygen content 21%) to obtain the highly dispersed copper-supported rod-shaped cerium-based catalyst for the efficient catalytic oxidation of CO.
[0094] Example 2
[0095] Select copper as the transition element load, take copper salt different from Example 1 as the precursor, and use rod-shaped cerium oxide nanoparticles synthesized by hydrothermal method as the carrier. The preparation steps of copper element highly dispersed loaded rod-shaped cerium-based (Cu / CeO2) catalyst are as follows:
[0096] Step 1: Weigh 1.000g of cerium oxide carrier, measure 40mL of deionized water, add CeO2 into the deionized water and stir vigorously, put the obtained suspension into an ultrasonic cleaner for 30 minutes to obtain a well-dispersed carrier suspension;
[0097] Step 2: Weigh 0.038 g of copper nitrate trihydrate, measure 40 mL of deionized water, dissolve the weighed copper nitrate trihydrate in the deionized water, and stir until completely dissolved to obtain a clear solution;
[0098] Step 3: Add the clarified solution obtained in step 2 to the suspension obtained in step 1, and stir vigorously at a speed of 450 r / min for 2 h to obtain a mixed solution;
[0099] Step 4: Transfer the mixed solution obtained in step 3 to a polytetrafluoroethylene reactor with a capacity of 100 ml, tighten the stainless steel hydrothermal reactor, and perform a hydrothermal reaction for 12 hours in a constant temperature oven preheated to 100°C;
[0100] Step 5: Filter and separate the solid treated in step 4, wash it with deionized water and ethanol in turn, dry it at 60°C overnight, and calcine it at 400°C for 4 hours in air (oxygen content 21%) to obtain a copper element highly dispersed supported rod-shaped cerium-based catalyst prepared using a different transition metal precursor from Example 1.
[0101] Comparative Example 1
[0102] The unsupported rod-shaped cerium oxide nanoparticle (CeO 2 ) catalyst, ie, the cerium oxide support used in step 1 of the embodiment, was directly used.
[0103] Catalytic activity test
[0104] Test conditions: The catalyst powders obtained in Example 1, Example 2 and Comparative Example 1 were tableted, crushed and sieved, and catalyst particles of 40-60 mesh were selected for catalytic oxidation of CO activity evaluation. 0.1 g of catalyst was mixed with 0.1 g of inert quartz sand. The total flow rate of the treated exhaust gas was 100 mL / min, the reaction space velocity was GHSV 60,000 mL / (gh), and the exhaust gas composition was CO 1 vol.%, O2 21 vol.%, N2 78 vol.% O2. The results are shown in Figure 1 .
[0105] from Figure 1It can be seen from the test results that the activity of the Cu / CeO2 catalysts of Example 1 and Example 2 in catalytic oxidation of CO increases rapidly with the increase of temperature, and the CO conversion rates at various operating temperatures of 130-250°C are significantly better than those of Comparative Example 1, with significantly lower activation temperatures and CO 90% conversion temperatures. Specifically, the CO 90% conversion temperature of Example 1 is about 125°C, and the CO 90% conversion temperature of Example 2 is about 150°C.
[0106] Microstructure testing
[0107] Example 1 and Comparative Example 1 were taken as examples for microstructure testing.
[0108] Figure 2 The transmission electron microscope image (a) and the spherical aberration corrected scanning transmission electron microscope image (b) of the Cu / CeO2 catalyst of Example 1, the X-ray diffraction spectrum (c) and the X-ray absorption fine structure spectrum (d) of the Cu / CeO2 catalyst of Example 1, and the Raman spectra (e) and (f) of the Cu / CeO2 catalyst of Example 1 and the CeO2 catalyst of Comparative Example 1.
[0109] Depend on Figure 2 It can be seen that Cu / CeO2 is a porous material formed by the accumulation of cerium dioxide grains loaded with copper elements, with uniform size and a single grain diameter of 5 to 10 nm;
[0110] Depend on Figure 2 a, 2c and 2d, it can be seen that Cu / CeO2 retains the structural morphology of the carrier CeO2, has a face-centered cubic fluorite structure, and the morphology is still rod-shaped;
[0111] Depend on Figure 2 b It can be seen that the Cu element on the Cu / CeO2 surface is distributed in sub-nanometer atomic clusters of 1 to 5 nm, and no agglomeration is observed;
[0112] Depend on Figure 2 From e and f, it can be seen that the copper element in the Cu / CeO2 of Example 1 is anchored on the oxygen vacancies of the cerium oxide carrier; while the CeO2 catalyst of Comparative Example 1 has no copper element anchored.
[0113] Cu / CeO2 provides more adsorption sites due to the uniform loading of highly dispersed copper elements. At the same time, the strong interaction between the loaded copper elements and the carrier cerium oxide improves the chemical properties and defect structure of the carrier surface and enhances the activity of the reaction sites.
[0114] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
[0115] Industrial Applicability
[0116] The catalyst of the present invention is composed of cerium dioxide (CeO2) loaded with transition metal elements, and highly dispersed sub-nanometer atomic clusters of transition metals are obtained on the surface of the CeO2 carrier, which has good atomic utilization and an electronic structure that is conducive to CO adsorption and reaction. The obtained transition metal element highly dispersed loaded cerium-based catalyst has excellent CO catalytic oxidation activity, reaching the level of existing commercial precious metal catalysts, and is simple to prepare, low in cost, and can be mass-produced, and can be widely used in the emission control of high-concentration CO in waste gases such as boiler flue gas, blast furnace flue gas, and coking flue gas.
Claims
1. A transition metal element supported cerium-based catalyst, characterized in that: The catalyst is a porous material composed of crystal grains formed by cerium dioxide as a carrier and a transition metal element. The catalyst is represented by the formula M / CeO2, wherein M is a transition metal element. The transition metal element is in the form of monodispersed sub-nanometer atomic clusters with a size of 1 to 5 nm on the surface of the cerium dioxide. The transition metal element is anchored on the oxygen vacancies on the surface of cerium dioxide as a carrier. The molar ratio of the transition metal element to the cerium dioxide is 1:5 to 1:200, The transition metal element supported cerium-based catalyst is obtained by a preparation method comprising the following steps: Step 1: dispersing the cerium dioxide carrier into the first solvent by ultrasonication to obtain a suspension; Step 2: dissolving a transition metal element precursor in a second solvent to obtain a clear solution; Step 3: adding the clarified solution obtained in step 2 to the suspension obtained in step 1 and stirring to obtain a mixed solution; Step 4: transferring the mixed solution obtained in step 3 to a hydrothermal reaction kettle for hydrothermal reaction; Step 5: Separate, wash, dry and calcine the solid obtained by the hydrothermal reaction in step 4 to obtain a transition metal element-supported cerium-based catalyst in which the transition metal element is supported on cerium dioxide as a carrier, wherein the calcination is calcined under an oxygen content of 1 to 21 vol%.
2. The catalyst according to claim 1, wherein The molar ratio of the transition metal element to the cerium dioxide is 1:20 to 1:
100.
3. The catalyst according to claim 1 or 2, wherein The diameter of the crystal grains is 5 to 100 nm; the pore size of the porous material is 5 to 100 nm; the BET surface area of the porous material is 5 to 150 m 2 ·g -1 .
4. The catalyst according to claim 1 or 2, wherein The diameter of the crystal grains is 5 to 20 nm; the pore size of the porous material is 5 to 20 nm; the BET surface area of the porous material is 50 to 1502-1 m.g.
5. The catalyst according to claim 1 or 2, wherein The transition metal element is selected from one or more of manganese, iron, cobalt, nickel and copper.
6. A method for preparing a transition metal element supported cerium-based catalyst according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: Step 1: dispersing the cerium dioxide carrier into the first solvent by ultrasonication to obtain a suspension; Step 2: dissolving a transition metal element precursor in a second solvent to obtain a clear solution; Step 3: adding the clarified solution obtained in step 2 to the suspension obtained in step 1 and stirring to obtain a mixed solution; Step 4: transferring the mixed solution obtained in step 3 to a hydrothermal reaction kettle for hydrothermal reaction; Step 5: Separate, wash, dry and calcine the solid obtained by the hydrothermal reaction in step 4 to obtain a transition metal element-supported cerium-based catalyst in which the transition metal element is supported on cerium dioxide as a carrier, wherein the calcination is calcined under an oxygen content of 1 to 21 vol%.
7. The preparation method according to claim 6, wherein: In the suspension in step one, the mass concentration of the cerium dioxide carrier is 5 to 200 g / L; the molar ratio of the transition metal element precursor used in step two to the cerium dioxide carrier used in step one is 1:5 to 1:200; in the clear solution, the molar concentration of the transition metal element precursor is 0.001 to 0.04 mol / L.
8. The preparation method according to claim 6, wherein: In the suspension in step one, the mass concentration of the cerium dioxide carrier is 20 to 100 g / L; the molar ratio of the transition metal element precursor used in step two to the cerium dioxide carrier used in step one is 1:20 to 1:100; in the clear solution, the molar concentration of the transition metal element precursor is 0.003 to 0.01 mol / L.
9. The preparation method according to any one of claims 6 to 8, wherein: The transition metal element precursor is selected from a mixture of one or more of manganese nitrate, manganese chloride, manganese sulfate, manganese acetate, manganese bromide, ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferrous sulfate, ferrous sulfate, ferrous acetate, ferrous acetate, ferric bromide, ferrous bromide, cobalt nitrate, cobalt chloride, cobalt sulfate, cobalt acetate, cobalt bromide, nickel nitrate, nickel chloride, nickel sulfate, nickel acetate, nickel bromide, copper nitrate, copper chloride, copper sulfate, copper acetate, and copper bromide; the first solvent and the second solvent are selected from a mixture of one or more of water, ethanol, methanol, ethylene glycol, and acetone; the first solvent and the second solvent are the same or different.
10. The preparation method according to any one of claims 6 to 8, wherein: In the step 1, the ultrasonic dispersion time is 1 to 200 minutes; in the step 3, the stirring time is 0.5 to 12 hours; in the step 4, the hydrothermal temperature is 50 to 150° C., and the hydrothermal time is 0.5 to 36 hours; in the step 5, the calcination temperature is 200 to 800° C., and the calcination time is 0.5 to 12 hours.
11. The preparation method according to any one of claims 6 to 8, wherein: In the step 1, the ultrasonic dispersion time is 20 to 100 minutes; in the step 3, the stirring time is 1 to 8 hours; in the step 4, the hydrothermal temperature is 80 to 120° C., and the hydrothermal time is 6 to 24 hours; in the step 5, the calcination temperature is 400 to 600° C., and the calcination time is 4 to 8 hours.
12. Use of the catalyst according to any one of claims 1 to 5 or the catalyst obtained by the preparation method according to any one of claims 6 to 11 for removing CO from exhaust gas.