A grinding preparation method of halogen-doped metal oxide nanozyme and its application
The preparation of halogen-doped metal oxide nanozymes by solid-phase mechanochemistry solves the problems of low catalytic efficiency and complex production in the existing technology, and realizes the preparation of efficient and environmentally friendly halogen-doped metal oxides, which is suitable for large-scale production. .
Patent Information
- Application Number
- CN202310048279.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-01-31
Smart Images

Figure CN115970713B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of inorganic functional material chemistry, and specifically relates to a grinding preparation method of a halogen-doped metal oxide nanozyme and an application thereof. Background Art
[0002] Nanozymes are a type of nanomaterials with enzyme activity. Compared with natural enzymes, they have the advantages of high stability, low cost, and recyclability. Since the nanozyme performance of ferroferric oxide was first reported in 2007, a variety of metal oxide nanomaterials with enzyme-like activity have been gradually discovered. Among them, metal oxides with peroxidase (POD)-like activity can activate hydrogen peroxide (H2O2) to produce reactive oxygen species such as hydroxyl radicals, which can be used in biosensing, antibacterial, cancer diagnosis and treatment, environmental monitoring, and wastewater treatment. However, the current application bottlenecks of metal oxides with POD-like activity are mainly concentrated on the low catalytic efficiency of the materials and the low specificity for the reaction substrates. To solve the above problems, existing research mainly modulates the POD-like properties of metal oxide nanozymes from the aspects of material morphology regulation and size modulation. Related research pays less attention to the modulation effect of halogen doping on the performance of metal oxide POD-like. Although recent studies have found that the adsorption of a certain amount of fluoride ions on the surface of cerium oxide can significantly improve its enzyme-like catalytic activity, this study only added halogen ions to the cerium oxide system under liquid phase catalytic conditions to achieve surface adsorption of halogen ions, and did not involve the doping of halogen ions in the bulk phase of the material [Nanoscale 2019, 38, 17841]. Recent studies have shown that halogen doping can effectively adjust the catalytic properties of metal oxides. For example, Xie Zhaoxiong et al. found that chlorine-doped cuprous oxide rhombic dodecahedron nanocrystals prepared by a one-step liquid phase method have higher catalytic conversion and selectivity for the direct epoxidation of propylene to ethylene oxide [JAm Chem Soc 2020, 33, 14134]; Li Haitao et al. found that chlorine-doped cuprous oxide increased the yield of 1,4-butynediol from 73% to 94% in the ethylation reaction of formaldehyde [Processes 2019, 4, 7]; Park Hyun-kyung et al. found that iodine-doped titanium dioxide showed good visible light catalytic activity in the degradation of diclofenac and wastewater treatment [Chemical Engineering Journal 2019, 968]. These research results show that halogen doping may be an effective means to modulate the POD-like properties of metal oxides.
[0003] On the other hand, the existing preparation methods of halogen-doped metal oxides mainly involve electrochemical deposition, one-step liquid phase synthesis, post-impregnation treatment of oxide precursors, hydrolysis, and sol-gel methods. Among them, the electrochemical deposition method has simple equipment, is easy to control, and does not require high temperature and high pressure, but most of the products are deposited on the electrode surface, the yield is low, and it is not conducive to large-scale preparation; although the solution synthesis method is simple to operate, the halogen doping rate is not high and it is not easy to scale up the preparation; and the samples obtained by post-impregnation treatment of metal oxides have poor stability, and there is a problem that the interaction between metal ions and halogen ions is not strong, and halogen ions are easy to lose; although the hydrolysis method is simple to operate, it requires a high temperature environment and is more dangerous; although the sol-gel method is easy to achieve uniform halogen doping at the molecular level, the reaction time is long, often requiring several days or weeks. Therefore, finding a more efficient, simple and suitable preparation method for halogen-doped metal oxides for actual production applications has important research significance and good market application prospects. Summary of the invention
[0004] The present invention aims to develop a method for preparing halogen-doped metal oxides, and obtain halogen-doped metal oxides with high-efficiency peroxidase-like activity by solid phase mechanochemical method.
[0005] A grinding preparation method for halogen-doped metal oxide nanozyme comprises the following steps:
[0006] At a temperature between 0 and 100° C., a metal precursor is mixed with a halogen precursor, and the mixture is manually ground or ball-milled. The resulting product is washed with deionized water and dried to obtain a halogen-doped metal oxide nanozyme. The temperature is preferably 20 to 80° C.
[0007] Furthermore, the drying is vacuum drying or drying, wherein the purpose of vacuum drying is to prevent oxidation of certain metal oxides. The drying temperature is 30-50° C. and the drying time is 6-8 hours.
[0008] Furthermore, the metal precursor is a metal oxide or a metal powder; the halogen precursor is one or a combination of alkali metal halides, alkaline earth metal halides, and ammonium halides.
[0009] Furthermore, the metal oxide is any one or a combination of several of copper oxide, cuprous oxide, zinc oxide, titanium dioxide, cobalt oxide, cobalt tetroxide, cobalt trioxide, ferrous oxide, ferric oxide, cerium dioxide, manganese dioxide, manganese tetroxide, manganese trioxide, aluminum oxide, molybdenum dioxide, molybdenum trioxide, vanadium pentoxide, nickel oxide, magnesium oxide, calcium oxide, barium oxide, tungsten trioxide, zirconium dioxide, ruthenium dioxide, tin dioxide, LaNiO3, LaCoO3, LaMnO3, and SrFeO3, and the corresponding metal oxide is a commercial metal oxide or a synthetic metal oxide; the metal powder is any one or a combination of several of copper powder, iron powder, cobalt powder, nickel powder, tin powder, molybdenum powder, tungsten powder, titanium powder, and vanadium powder.
[0010] Furthermore, in step 1, the molar ratio of the metal in the metal precursor to the halogen ion in the halogen precursor is 1:0.1-8. When the molar ratio of the metal to the halogen ion is greater than 1:8, metal halide is easily generated.
[0011] Furthermore, the manual grinding reaction time is 10 to 60 minutes; the ball milling reaction time is 5 minutes to 12 hours; the manual grinding is to grind the mixture manually in a mortar; the ball milling is to add the mixture and grinding balls into a ball mill jar for mechanical grinding.
[0012] Furthermore, the mass ratio of the ball to the material in the ball milling reaction is 10 to 30:1; and the atmosphere of the ball milling reaction is one of air, nitrogen, argon or vacuum.
[0013] Furthermore, the grinding balls are zirconia balls or stainless steel balls, the diameter of the grinding balls is 3 to 40 mm, preferably 3 to 10 mm, and the density of the grinding balls is not less than 6 g / cm 3 ; The rotation speed of the ball mill is 0~1000rpm.
[0014] The peroxidase-like catalytic conditions of a material prepared by a grinding preparation method of a halogen-doped metal oxide nanozyme are evaluated in a solution containing substrates 3,3',5,5'-tetramethylbenzidine and hydrogen peroxide to catalyze and activate hydrogen peroxide and promote the oxidation of the substrate.
[0015] A peroxidase-like catalytic application of a material obtained by a grinding preparation method of a halogen-doped metal oxide nanozyme, and applications of the peroxidase-like catalytic performance of the material in antibacterial and dye degradation, wherein the antibacterial application is to evaluate the inhibitory effect of the halogen-doped metal oxide nanozyme on drug-resistant Staphylococcus aureus by counting the number of colonies through a plate coating method in an acidic environment; the dye degradation application is to evaluate the performance of the halogen-doped metal oxide nanozyme in degrading dyes by comparing the changes in absorbance before and after degradation of organic dyes such as rhodamine B and methyl orange in an acidic environment.
[0016] The beneficial effects of the present invention are:
[0017] (1) Halogen doping significantly enhances the peroxidase-like catalytic activity of metal oxide nanozymes, resulting in them exhibiting excellent antibacterial properties and catalytic oxidative dye degradation properties.
[0018] (2) The halogen doping amount of the product increases with the amount of halogen precursor added during preparation, making it easy to prepare metal oxide nanozymes with high halogen doping amounts. Moreover, this method saves solvent, has high yield, is easy to scale up, and is suitable for large-scale production.
[0019] (3) The process is simple, the operation is easy, and the reaction conditions are mild.
[0020] (4) The preparation cost is low, the energy consumption is low, and no harmful waste is generated, which meets the modern production requirements of "green production, environmental protection and energy saving". BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The XRD spectra of commercial cuprous oxide and chlorine-doped commercial cuprous oxide are shown below;
[0022] Figure 2 It is a local enlarged view of the XRD (111) diffraction peak of commercial cuprous oxide and chlorine-doped commercial cuprous oxide;
[0023] Figure 3 This is the TEM image of commercial cuprous oxide;
[0024] Figure 4 This is a TEM image of chlorine-doped commercial cuprous oxide;
[0025] Figure 5 The XPS diagram of Cl 2p of chlorine-doped commercial cuprous oxide;
[0026] Figure 6 Fluorescence spectra of hydroxyl radicals generated by the decomposition of H2O2 catalyzed by commercial cuprous oxide and chlorine-doped commercial cuprous oxide using terephthalic acid;
[0027] Figure 7is a comparison of the peroxidase-like (POD) activity of chlorine-doped commercial cuprous oxide and commercial cuprous oxide in a solution in the presence of 3,3',5,5'-tetramethylbenzidine (TMB) and hydrogen peroxide (H2O2) (POD-like activity increase factor = absorbance increase rate of halogen-doped metal oxide at 652 nm / absorbance increase rate of metal oxide at 652 nm);
[0028] Figure 8 POD-like catalytic activity of chlorine-doped commercial cuprous oxide at different (a) pH and (b) temperatures.
[0029] Fig. 9 The XRD patterns of nano-octahedral cuprous oxide and chlorine-doped nano-octahedral cuprous oxide;
[0030] Fig.10 It is a local enlarged view of the XRD (111) diffraction peak of nano-octahedral cuprous oxide and chlorine-doped nano-octahedral cuprous oxide;
[0031] Fig.11 To compare the POD activities of chlorine-doped nano-octahedral cuprous oxide and nano-octahedral cuprous oxide in the presence of TMB and H2O2;
[0032] Fig.12 Fluorescence spectra of hydroxyl radicals generated by commercial cobalt tetroxide captured by terephthalic acid and chlorine-doped commercial cobalt tetroxide catalyzed decomposition of H2O2;
[0033] Fig.13 To compare the POD-like activity of fluorine-doped commercial cobalt tetroxide and commercial cobalt tetroxide in the presence of TMB and H2O2;
[0034] Fig.14 Fluorescence spectra of hydroxyl radicals generated by the decomposition of H2O2 catalyzed by commercial titanium dioxide and chlorine-doped commercial titanium dioxide using terephthalic acid;
[0035] Fig.15 To compare the POD-like activity of chlorine-doped commercial TiO2 and commercial TiO2 in the presence of TMB and H2O2;
[0036] Fig.16 This is a comparison of the POD-like activity of commercial cuprous oxide doped with different amounts of chlorine. The percentage sign in the name of the chlorine-doped samples represents the percentage of the mass of sodium chloride used in the preparation to the total mass of sodium chloride and commercial cuprous oxide;
[0037] Fig.17The C / C0 change curve of the time tracking of the oxidative degradation of the organic dye Rhodamine B by commercial cuprous oxide and chlorine-doped commercial cuprous oxide, wherein C is the concentration of Rhodamine B at a fixed time point, and C0 is the initial concentration of Rhodamine B;
[0038] Fig.18 The C / C0 change curve of the time tracking of the oxidative degradation of the organic dye methyl orange by commercial cuprous oxide and chlorine-doped commercial cuprous oxide, wherein C is the concentration of methyl orange at a fixed time point, and C0 is the initial concentration of methyl orange;
[0039] Fig.19 The C / C0 curves of the time-tracking oxidative degradation of the organic dye methyl orange by commercial cobalt tetroxide and chlorine-doped commercial cobalt tetroxide, where C is the concentration of methyl orange at a fixed time point and C0 is the initial concentration of methyl orange;
[0040] Fig. 20 Plate images of drug-resistant Staphylococcus aureus treated with different concentrations of commercial cuprous oxide and chlorine-doped commercial cuprous oxide as well as a control group;
[0041] Fig.21 (a) Plate images of drug-resistant Staphylococcus aureus after treatment under different conditions; (b) Statistical colony counts under corresponding experimental conditions. DETAILED DESCRIPTION
[0042] The present invention will be further described below by way of embodiments in conjunction with the accompanying drawings.
[0043] Example 1
[0044] 36 mg of sodium chloride and 200 mg of commercial cuprous oxide were added to a mortar and stirred evenly at 25° C. The mixture was manually ground for 40 min. The obtained product was washed with deionized water and dried under vacuum at 50° C. for 6 h to obtain chlorine-doped commercial cuprous oxide.
[0045] Test conditions for the POD-like activity of materials: In a solution containing the reducing substrates TMB and H2O2, the absorbance of the single-electron oxidation product obtained by the decomposition of H2O2 catalyzed by commercial cuprous oxide before and after chlorine doping was detected to change with time at 652nm. The absorbance growth rate of the product under the catalysis of the two materials was compared to evaluate the effect of halogen doping on the POD-like activity of commercial cuprous oxide. The specific conditions for detecting the POD-like catalytic activity are as follows: At 25°C, 10uL of 0.4mg / mL catalyst, 20uL of 50mM TMB and 50uL of 10M H2O2 were added to 920uL of acetic acid-sodium acetate buffer (pH=3.6), reacted for 1min, and UV test was performed.
[0046] XRD patterns of commercial cuprous oxide before and after chlorine doping Figure 1-2 shown. Figure 1 This indicates that the crystal structure of the material remains unchanged after doping, and it is still cuprous oxide. However, the diffraction peak moves toward the low diffraction angle as a whole. This indicates that since the radius of chloride ions is larger than that of oxygen ions, doping causes the lattice of the material to expand, causing the diffraction peak to move toward the low angle direction. Figure 2 Taking the (111) diffraction peak of cuprous oxide as an example, the Bragg formula was used to calculate that the lattice expansion rate caused by chlorine doping was 0.28%. Figure 3-4 They are TEM images of commercial cuprous oxide and chlorine-doped commercial cuprous oxide respectively. Figure 3-4 It shows that after chlorine doping, the morphology of commercial cuprous oxide remains basically unchanged. Figure 5 The Cl 2p photoelectron spectroscopy of chlorine-doped commercial cuprous oxide can be used to obtain the Cl 2p 3 / 2 Peak 197.8eV and Cl 2p 1 / 2 The peak 199.4eV is 1.6eV apart, and the ratio of the peak areas is about 2:1, which indicates that chloride ions enter the Cu2O lattice, replacing lattice oxygen atoms and combining with copper atoms. Figure 6 The data show that chlorine-doped commercial cuprous oxide has an enhanced ability to catalyze the decomposition of H2O2 to produce hydroxyl radicals compared to commercial cuprous oxide. Figure 7 The POD-like catalytic data of the materials in the study showed that the POD-like activity of chlorine-doped commercial cuprous oxide was increased by 2.5 times compared with commercial cuprous oxide.
[0047] Figure 8 The POD-like activity of chlorine-doped commercial cuprous oxide at different pH and temperature when other test conditions remained the same. Figure 8 The data in (a) show that when other conditions remain the same, the POD-like activity of the material is different in different pH environments. When pH = 3.6, its enzyme-like activity is the highest. Figure 8 The data in (b) show that when other conditions remain the same, the material has different POD-like activities at different temperatures. When the temperature is 45°C, its enzyme-like activity is the highest.
[0048] Example 2
[0049] Add 2mmol copper nitrate and 0.7g polyvinyl pyrrolidone to the serum bottle, stir the reaction mixture at 55°C, and after the polyvinyl pyrrolidone is completely dissolved, add 6mL 1M sodium hydroxide and 2mL 0.6M ascorbic acid, and react for 30min. Centrifuge at 8000rpm for 10min, wash repeatedly with deionized water, ethanol and acetone for more than three times, and vacuum dry at 50°C for 6h to obtain nano octahedral cuprous oxide.
[0050] 18 mg of ammonium chloride and 100 mg of nano-octahedral cuprous oxide were added to a mortar, stirred evenly at 25° C., and the mixture was manually ground for 40 min. The obtained product was washed with deionized water and vacuum dried at 50° C. for 6 h to obtain chlorine-doped nano-octahedral cuprous oxide. The POD-like activity test conditions were consistent with those in Example 1, and the POD-like activity of nano-octahedral cuprous oxide before and after chlorine doping was evaluated.
[0051] XRD patterns of nano-octahedral cuprous oxide before and after chlorine doping Figure 9-10 shown. Fig. 9 This shows that the crystal structure of the material remains unchanged after doping, and it is still cuprous oxide. However, the diffraction peak moves toward the low diffraction angle as a whole. This shows that since the radius of chloride ions is larger than that of oxygen ions, doping causes the lattice of the material to expand, thus causing the diffraction peak to move toward the low angle direction. Fig.10 As shown in Figure 2, taking the (111) diffraction peak as an example, the Bragg formula is used to calculate that chlorine doping causes the lattice to expand by 0.26%. Compared with nano-octahedral cuprous oxide, the POD-like activity of chlorine-doped nano-octahedral cuprous oxide is increased by 2.1 times, as shown in Figure 2. Fig.11 shown.
[0052] Example 3
[0053] 36 mg of potassium fluoride and 200 mg of commercial cobalt tetroxide were added to a mortar, stirred evenly at 30°C, and the mixture was manually ground for 10 minutes. The obtained product was washed with deionized water and vacuum dried at 40°C for 7 hours to obtain fluorine-doped commercial cobalt tetroxide. The POD-like activity test conditions were consistent with those in Example 1, and the POD-like activity of commercial cobalt tetroxide before and after fluorine doping was evaluated.
[0054] Fig.12 It can be seen that the ability of fluorine-doped commercial cobalt tetroxide to activate hydrogen peroxide is enhanced, producing more hydroxyl radicals. Fig.13 It shows that the POD-like activity of fluorine-doped commercial cobalt tetroxide is increased by 1.7 times compared with commercial cobalt tetroxide.
[0055] Example 4
[0056] Add 100 mg of calcium chloride and 100 mg of commercial titanium dioxide into a zirconia ball mill, then add 5 mm diameter zirconia grinding balls and 8 mm diameter zirconia grinding balls. The ball-to-material mass ratio is 10:1. The density of the grinding balls is not less than 6 g / cm 3 (The grinding ball density selected in the subsequent examples is not less than 6g / cm 3). The reaction temperature was set to 55°C, the speed of the ball mill was set to 600 rpm, and mechanical grinding was performed in an air atmosphere for 5 minutes. The obtained product was washed with deionized water and vacuum dried at 45°C for 6 hours to obtain chlorine-doped commercial titanium dioxide. The POD-like activity test conditions were consistent with those in Example 1, and the POD-like activity of commercial titanium dioxide before and after chlorine doping was evaluated.
[0057] Fig.14 It can be seen that the ability of chlorine-doped commercial titanium dioxide to activate hydrogen peroxide is enhanced, producing more hydroxyl radicals. Fig.15 It shows that the POD-like activity of chlorine-doped commercial titanium dioxide is increased by 1.2 times compared with commercial titanium dioxide.
[0058] Example 5
[0059] Different masses of sodium chloride and 100 mg of commercial cuprous oxide were added to a polytetrafluoroethylene ball mill jar, respectively, wherein the mass of sodium chloride accounted for 15%, 30%, 45%, 60% and 75% of the total mass of sodium chloride and commercial cuprous oxide, respectively. Then zirconium oxide grinding balls with a diameter of 5 mm and zirconium oxide grinding balls with a diameter of 8 mm were added, and the ball-to-material mass ratio was 10:1. The reaction temperature was set to 30°C, the ball mill speed was 600 rpm, and mechanical grinding was performed under vacuum conditions for 20 minutes. The obtained solid product was washed with deionized water and dried in a vacuum at 50°C for 6 hours to obtain commercial cuprous oxide doped with different doping amounts of chlorine. The POD-like activity of commercial cuprous oxide doped with different doping amounts of chlorine was evaluated in accordance with the POD-like activity test conditions in Example 1, as shown in FIG. Fig.16 As shown in the figure, after chlorine doping, the POD-like activity of commercial cuprous oxide increases. The sample with a mass percentage of 15% of sodium chloride to the total mass of sodium chloride and commercial cuprous oxide has the highest POD-like activity, and then as the halogen doping amount during preparation increases from 15% to 75%, the POD-like activity of the catalyst shows a gradual downward trend.
[0060] Example 6
[0061] 100uL 2mg / mL organic dye Rhodamine B was added to 20mL deionized water, the pH of the system was adjusted to 3.6 with sulfuric acid, and 1mg commercial cuprous oxide or chlorine-doped commercial cuprous oxide and 200uL 10M H2O2 were added thereto, and the mixture was stirred continuously, and samples were taken every half an hour, centrifuged, and the absorbance of the liquid sample at 554nm was detected. By comparing the changes in absorbance before and after the degradation of Rhodamine B, a spectrum of the rate of oxidative degradation of Rhodamine B by commercial cuprous oxide and chlorine-doped commercial cuprous oxide was obtained. Fig.17It shows that when the reaction time reaches 150 minutes, the degradation rate of commercial cuprous oxide to rhodamine B is 75%, while the degradation rate of chlorine-doped commercial cuprous oxide to rhodamine B is almost 100%. This shows that chlorine doping can increase the rate of commercial cuprous oxide-catalyzed oxidative degradation of rhodamine B.
[0062] Example 7
[0063] Add 100uL of 2mg / mL organic dye methyl orange to 20mL of deionized water, adjust the pH of the system to 4 with sulfuric acid, add 15mg of commercial cuprous oxide or chlorine-doped commercial cuprous oxide and 200uL of 10M H2O2, stir continuously, take samples every half an hour, centrifuge, and detect the absorbance of the liquid sample at 465nm. By comparing the changes in absorbance before and after the degradation of methyl orange, the spectrum of the rate of catalytic oxidation degradation of methyl orange by commercial cuprous oxide and chlorine-doped commercial cuprous oxide is obtained. Fig.18 It can be seen that the degradation rate of methyl orange dye by chlorine-doped commercial cuprous oxide is greater than that of commercial cuprous oxide during the reaction. When the reaction is carried out for 180 minutes, the degradation rate of methyl orange by commercial cuprous oxide reaches 50%, while the degradation rate of methyl orange by chlorine-doped commercial cuprous oxide reaches 75%. Therefore, the comparison of the data of the two shows that chlorine doping can increase the rate of methyl orange degradation by commercial cuprous oxide catalytic oxidation.
[0064] Example 8
[0065] 100uL of 2mg / mL organic dye methyl orange was added to 20mL of deionized water, and the pH of the system was adjusted to 6 with sulfuric acid, and 20mg of commercial cobalt tetroxide or chlorine-doped commercial cobalt tetroxide and 200uL of 10M H2O2 were added thereto, and the mixture was stirred continuously, and samples were taken every half an hour, centrifuged, and the absorbance of the liquid sample at 465nm was detected. By comparing the changes in absorbance before and after the degradation of methyl orange, a spectrum of the rate of catalytic oxidation degradation of methyl orange by commercial cobalt tetroxide and chlorine-doped commercial cobalt tetroxide was obtained. Fig.19 It shows that when the reaction is carried out for 150 minutes, the degradation rate of methyl orange by commercial cobalt tetroxide is only 18%, while the degradation rate of methyl orange by chlorine-doped commercial cobalt tetroxide is 37%. Therefore, the comparison of the data of the two shows that chlorine doping can increase the rate of catalytic oxidation degradation of methyl orange by commercial cobalt tetroxide.
[0066] Example 9
[0067] Evaluation of the in vitro bactericidal properties of commercial cuprous oxide and chlorine-doped commercial cuprous oxide. First, the activated drug-resistant Staphylococcus aureus (MRSA) colonies were picked and cultured in LB liquid medium (200 rpm, 37°C) for 12 h. Subsequently, the culture medium was removed by centrifugation (3500 rpm, 5 min), and then washed three times with PBS buffer at pH 4, and finally MRSA was resuspended in PBS buffer solution. Secondly, MRSA (1×10 5 CFU / mL), PBS (10mM, 20μL), H2O2 (final concentration is 500μM) were incubated with different concentrations of commercial cuprous oxide (Cu2O) and chlorine-doped commercial cuprous oxide (Cl-Cu2O) (final concentrations were 50ug / mL, 100ug / mL, 200ug / mL, 500ug / mL) for 10 minutes. Finally, 20μL of the 100-fold diluted bacterial suspension was transferred to a solid LB agar plate and incubated at 37°C for 12h. The number of CFU was counted according to the colony distribution on the agar plate to investigate the bactericidal performance of different concentrations of Cu2O and Cl-Cu2O against MRSA.
[0068] Fig. 20 It shows that compared with the control group, low concentrations of Cu2O and Cl-Cu2O have no obvious inhibitory effect on MRSA. When the concentration reaches 200ug / mL, the MRSA growth activity of the Cu2O treatment group did not change significantly. In the Cl-Cu2O treatment group, the number of MRSA colonies decreased significantly, and when the material concentration was as high as 500ug / mL, its inhibitory efficiency on MRSA could almost reach 100%. This shows that Cl-Cu2O can kill bacteria more effectively than Cu2O, and the higher the concentration of Cl-Cu2O, the more obvious the antibacterial effect.
[0069] Example 10
[0070] Evaluation of the effects of halogen doping and added H2O2 on the in vitro bactericidal properties of commercial cuprous oxide. First, the activated drug-resistant Staphylococcus aureus (MRSA) colonies were picked and cultured in LB liquid medium (200 rpm, 37°C) for 12 hours. Subsequently, the culture medium was removed by centrifugation (3500 rpm, 5 min), and then washed three times with PBS buffer with a pH value of 4, and finally MRSA was resuspended in PBS buffer solution. Secondly, different treatment groups were set up: PBS control group, H2O2 (500 μM) control group, Cu2O (200 ug / mL) treatment group, Cl-Cu2O (200 ug / mL) treatment group, Cu2O (200 ug / mL) + H2O2 (500 μM) treatment group, Cl-Cu2O (200 ug / mL) + H2O2 (500 μM) treatment group, and Cl-Cu2O (200 ug / mL) + H2O2 (500 μM) treatment group, respectively, with MRSA (1×105 CFU / mL) and incubated for 10 min. Finally, the plate culture method was used to examine the growth of MRSA in different treatment groups to intuitively understand the bactericidal effects of different treatment groups on MRSA.
[0071] Fig.21 (a) shows that in the absence of H2O2, there is basically no significant difference in the growth activity of MRSA in the Cu2O treatment group and the Cl-Cu2O treatment group, and their colony counts are basically similar, such as Fig.21 (b) This result shows that the simple material treatment has no obvious bactericidal effect. The growth of MRSA in the Cu2O+H2O2 treatment group was not greatly affected, but the growth of MRSA was significantly inhibited after the Cl-Cu2O+H2O2 treatment, and the number of colonies was significantly reduced, as shown in Figure 2. Fig.21 (b) This indicates that chlorine doping enhances the ability of cuprous oxide to activate hydrogen peroxide, producing more hydroxyl radicals, thereby effectively achieving an antibacterial effect.
[0072] Embodiment 11
[0073] 100 mg of magnesium chloride, 50 mg of ammonium bromide and 100 mg of commercial copper oxide were added to a mortar, stirred evenly at 35°C, and the mixture was manually ground for 50 minutes. The obtained product was washed with deionized water and vacuum dried at 40°C for 7 hours to obtain commercial copper oxide co-doped with chlorine and bromine.
[0074] Example 12
[0075] 300 mg of sodium iodide and 200 mg of commercial copper oxide were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 30:1. The reaction temperature was set to 25°C, the ball mill speed was set to 1000 rpm, and mechanical grinding was performed in a nitrogen atmosphere for 5 hours. The obtained solid product was washed with deionized water and vacuum dried at 45°C for 6 hours to obtain iodine-doped commercial copper oxide.
[0076] Embodiment 13
[0077] 50 mg of sodium fluoride and 100 mg of commercial titanium dioxide were added to a mortar, stirred evenly at 35° C., and the mixture was manually ground for 30 min. The obtained product was washed with deionized water and vacuum dried at 50° C. for 6 h to obtain fluorine-doped commercial titanium dioxide.
[0078] Embodiment 14
[0079] 150 mg of calcium bromide, 100 mg of sodium iodide and 100 mg of commercial titanium dioxide were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 25:1. The reaction temperature was set to 25 ° C, the ball mill speed was 1000 rpm, and mechanical grinding was performed in a nitrogen atmosphere for 6 hours. The obtained solid product was washed with deionized water and vacuum dried at 35 ° C for 8 hours to obtain commercial titanium dioxide co-doped with bromine and iodine.
[0080] Embodiment 15
[0081] Add 50 mg of ammonium bromide and 100 mg of commercial zinc oxide into a polytetrafluoroethylene ball mill, and then add stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm, with a ball-to-material mass ratio of 20:1. Set the reaction temperature to 45°C, control the speed of the ball mill to 800 rpm, and grind mechanically in a nitrogen atmosphere for 1 hour. The obtained solid product is washed with deionized water and dried at 50°C for 6 hours to obtain bromine-doped commercial zinc oxide.
[0082] Example 16
[0083] 100 mg of calcium chloride and 200 mg of commercial ferrosoferric oxide were added to a mortar, stirred evenly at 25° C., and the mixture was manually ground for 40 min. The obtained product was washed with deionized water and dried at 40° C. for 7 h to obtain chlorine-doped commercial ferrosoferric oxide.
[0084] Embodiment 17
[0085] 100 mg of magnesium chloride and 100 mg of commercial cerium dioxide were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 15:1. The reaction temperature was set to 50°C, the speed of the ball mill was controlled to 600 rpm, and mechanical grinding was performed in a nitrogen atmosphere for 20 minutes. The obtained solid product was washed with deionized water and vacuum dried at 45°C for 6 hours to obtain chlorine-doped commercial cerium dioxide.
[0086] Embodiment 18
[0087] 36 mg of sodium fluoride, 50 mg of calcium chloride and 100 mg of commercial cerium dioxide were added to a mortar, stirred evenly at 25° C., and the mixture was manually ground for 40 minutes. The obtained product was washed with deionized water and vacuum dried at 45° C. for 6 hours to obtain fluorine- and chlorine-co-doped commercial cerium dioxide.
[0088] Embodiment 19
[0089] 50 mg of sodium iodide and 200 mg of commercial ferric oxide were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 25:1. The reaction temperature was set to 50 ° C, the speed of the ball mill was controlled to 1000 rpm, and mechanical grinding was performed in an argon atmosphere for 10 hours. The obtained solid product was washed with deionized water and vacuum dried at 50 ° C for 6 hours to obtain iodine-doped commercial ferric oxide.
[0090] Embodiment 20
[0091] 50 mg of sodium fluoride and 100 mg of commercial manganese dioxide were added to a mortar, stirred evenly at 30° C., and the mixture was manually ground for 30 min. The obtained product was washed with deionized water and dried at 40° C. for 8 h to obtain fluorine-doped commercial manganese dioxide.
[0092] Embodiment 21
[0093] 150 mg of magnesium bromide and 200 mg of commercial aluminum oxide were added to a polytetrafluoroethylene ball mill, followed by 5 mm diameter zirconium oxide grinding balls and 8 mm diameter zirconium oxide grinding balls, with a ball-to-material mass ratio of 30:1. The reaction temperature was set to 70°C, the speed of the ball mill was controlled to 800 rpm, and mechanical grinding was performed in an air atmosphere for 3 hours. The obtained solid product was washed with deionized water and dried at 35°C for 8 hours to obtain bromine-doped commercial aluminum oxide.
[0094] Embodiment 22
[0095] 150 mg of sodium iodide and 200 mg of commercial molybdenum dioxide were added to a mortar, stirred evenly at 25° C., manually ground for 60 min, washed with deionized water, and dried at 40° C. for 7 h to obtain iodine-doped commercial molybdenum dioxide.
[0096] Embodiment 23
[0097] 36 mg of ammonium chloride, 50 mg of calcium bromide and 100 mg of commercial molybdenum dioxide were added to a polytetrafluoroethylene ball mill, and then 5 mm diameter zirconium oxide grinding balls and 8 mm diameter zirconium oxide grinding balls were added, with a ball-to-material mass ratio of 25:1. The reaction temperature was set to 50 ° C, the speed of the ball mill was controlled to 800 rpm, and mechanical grinding was performed in an air atmosphere for 4 hours. The obtained solid product was washed with deionized water and dried at 45 ° C for 6 hours to obtain chlorine-bromine co-doped commercial molybdenum dioxide.
[0098] Embodiment 24
[0099] 50 mg of sodium fluoride and 100 mg of commercial vanadium pentoxide were added to a mortar, stirred evenly at 25° C., and the mixture was manually ground for 30 minutes. The obtained product was washed with deionized water and dried at 50° C. for 6 hours to obtain fluorine-doped commercial vanadium pentoxide.
[0100] Embodiment 25
[0101] 150 mg of magnesium chloride and 200 mg of commercial nickel oxide were added to a zirconia ball mill jar, followed by 5 mm diameter zirconia grinding balls and 8 mm diameter zirconia grinding balls, with a ball-to-material mass ratio of 30:1. The reaction temperature was set at 50°C, the speed of the ball mill was controlled at 600 rpm, and mechanical grinding was performed under air atmosphere for 1 hour. The obtained solid product was washed with deionized water and dried at 30°C for 8 hours to obtain chlorine-doped commercial nickel oxide.
[0102] Embodiment 26
[0103] Add 150 mg of sodium iodide and 100 mg of commercial magnesium oxide to a zirconia ball mill jar, and then add zirconia grinding balls with a diameter of 5 mm and zirconia grinding balls with a diameter of 8 mm, with a ball-to-material mass ratio of 20:1. Set the reaction temperature to 55°C, control the speed of the ball mill to 1000 rpm, and mechanically grind for 12 hours under vacuum conditions. The obtained solid product is washed with deionized water and dried at 40°C for 6 hours to obtain iodine-doped commercial magnesium oxide.
[0104] Embodiment 27
[0105] 150 mg of ammonium bromide and 100 mg of commercial calcium oxide were added to a mortar, stirred evenly at 30° C., and the mixture was manually ground for 50 min. The obtained product was washed with deionized water and dried at 45° C. for 6 h to obtain bromine-doped commercial calcium oxide.
[0106] Embodiment 28
[0107] Add 100 mg of sodium iodide and 200 mg of commercial barium oxide to a zirconia ball mill, and then add zirconia grinding balls with a diameter of 5 mm and zirconia grinding balls with a diameter of 8 mm, with a ball-to-material mass ratio of 20:1. Set the reaction temperature to 60°C, control the speed of the ball mill to 1000 rpm, and grind mechanically for 12 hours in an air atmosphere. Wash the solid product with deionized water and dry it at 35°C for 8 hours to obtain iodine-doped commercial barium oxide.
[0108] Embodiment 29
[0109] Add 100 mg of magnesium chloride and 200 mg of commercial tungsten trioxide into a mortar, stir evenly at 30°C, grind manually for 40 minutes, wash with deionized water, and dry at 50°C for 6 hours to obtain chlorine-doped commercial tungsten trioxide.
[0110] Embodiment 30
[0111] 50 mg of sodium fluoride and 100 mg of commercial zirconium dioxide were added to a mortar, stirred evenly at 25° C., and the mixture was manually ground for 60 min. The obtained product was washed with deionized water and dried at 45° C. for 7 h to obtain fluorine-doped commercial zirconium dioxide.
[0112] Embodiment 31
[0113] 150 mg of sodium iodide and 100 mg of commercial ruthenium dioxide were added to a polytetrafluoroethylene ball mill, followed by 5 mm diameter zirconium oxide grinding balls and 8 mm diameter zirconium oxide grinding balls, with a ball-to-material mass ratio of 15:1. The reaction temperature was set to 50 ° C, the speed of the ball mill was controlled to 1000 rpm, and mechanical grinding was performed under nitrogen atmosphere for 2 hours. The obtained solid product was washed with deionized water and dried at 50 ° C for 6 hours to obtain iodine-doped commercial ruthenium dioxide.
[0114] Embodiment 32
[0115] 450 mg of lanthanum nitrate hexahydrate, 300 mg of nickel nitrate hexahydrate and 200 mg of citric acid as a complexing agent were dissolved in deionized water, heated and stirred for a certain period of time, and then placed in an oven for drying and dehydration to obtain a fluffy precursor complex. After grinding it into a powder without obvious granularity, it was placed in a porcelain crucible and moved to a muffle furnace. After calcination in an air atmosphere, it was cooled with the furnace temperature to obtain a black LaNiO3 powder.
[0116] 50 mg of sodium fluoride and 100 mg of LaNiO3 were added to a mortar and stirred evenly at 25°C. The mixture was manually ground for 30 min. The obtained product was washed with deionized water and vacuum dried at 30°C for 8 h to obtain fluorine-doped LaNiO3.
[0117] Embodiment 33
[0118] 450 mg of lanthanum nitrate hexahydrate and 300 mg of cobalt nitrate hexahydrate were dissolved in deionized water, and 200 mg of citric acid was added thereto. The pH value was adjusted to 10 with aqueous ammonia, and the mixture was stirred thoroughly and allowed to stand. When the mixture formed a gel, it was calcined at 50°C for 2 hours to obtain LaCoO3 powder.
[0119] 36 mg of sodium bromide and 200 mg of LaCoO3 were added to a polytetrafluoroethylene ball mill, followed by 5 mm diameter zirconium oxide grinding balls and 8 mm diameter zirconium oxide grinding balls, with a ball-to-material mass ratio of 10:1. The reaction temperature was set to 60°C, the speed of the ball mill was controlled to 800 rpm, and mechanical grinding was performed in a nitrogen atmosphere for 30 min. The obtained solid product was washed with deionized water and vacuum dried at 35°C for 7 h to obtain bromine-doped LaCoO3.
[0120] Embodiment 34
[0121] 450 mg of lanthanum nitrate hexahydrate and 321 mg of manganese nitrate hexahydrate were mixed and dissolved in a certain amount of deionized water, placed in a heat-collecting constant temperature heating magnetic stirrer and stirred to dissolve, 60 mg of precipitant urea was gradually added, and after continuous stirring to dissolve, it was transferred to a high-pressure reactor, reacted in an oven at 120°C for 2 hours, cooled to room temperature, filtered and washed, the precipitate was dried at 120°C for 2 hours, and calcined in a muffle furnace at 700°C for 6 hours to obtain LaMnO3 powder.
[0122] 50 mg of calcium chloride and 200 mg of LaMnO3 were added to a mortar and stirred evenly at 30°C. The mixture was manually ground for 40 min. The obtained product was washed with deionized water and dried under vacuum at 40°C for 6 h to obtain chlorine-doped LaMnO3.
[0123] Embodiment 35
[0124] 810 mg of ferric nitrate nonahydrate and 420 mg of strontium nitrate were dissolved in deionized water, and 200 mg of citric acid was added thereto. After being fully stirred, the mixture was dried under an infrared lamp until a sol was formed. After being allowed to stand to form a gel, the mixture was vacuum dried to obtain SrFeO3 dry gel.
[0125] 150 mg of potassium iodide and 200 mg of SrFeO3 were added to a mortar and stirred evenly at 25°C. The mixture was manually ground for 60 min. The obtained product was washed with deionized water and vacuum dried at 40°C for 6 h to obtain iodine-doped SrFeO3.
[0126] Embodiment 36
[0127] 300 mg of sodium iodide, 200 mg of commercial cuprous oxide and 200 mg of commercial ferric oxide were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, and the ball-to-material mass ratio was 30:1. The reaction temperature was set to 50°C, the speed of the ball mill was controlled to 1000 rpm, and mechanical grinding was performed in an argon atmosphere for 12 hours. The obtained solid product was washed with deionized water and vacuum dried at 45°C for 6 hours to obtain a composite of iodine-doped commercial cuprous oxide and iodine-doped commercial ferric oxide.
[0128] Embodiment 37
[0129] 500 mg of commercial copper powder was added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 30:1. The reaction temperature was set to 40°C, the speed of the ball mill was controlled to 800 rpm, and mechanical grinding was performed in an air atmosphere for 40 minutes, and oxidation reaction occurred in full contact with air to obtain cuprous oxide.
[0130] 36 mg of sodium chloride and 200 mg of cuprous oxide prepared in the previous step were added to a polytetrafluoroethylene ball mill, and then 5 mm diameter zirconium oxide grinding balls and 8 mm diameter zirconium oxide grinding balls were added, and the ball-to-material mass ratio was 15:1. The reaction temperature was set to 30 ° C, the ball mill speed was 600 rpm, and mechanical grinding was performed under vacuum for 5 h. The obtained solid product was washed with deionized water and vacuum dried at 30 ° C for 8 h to obtain chlorine-doped cuprous oxide.
[0131] Embodiment 38
[0132] 300 mg of commercial copper powder was added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 25:1. The reaction temperature was set to 80°C, the speed of the ball mill was controlled to 1000 rpm, and mechanical grinding was performed in an air atmosphere for 4 hours to fully contact with the air for oxidation reaction to obtain copper oxide.
[0133] 18 mg of ammonium chloride and 100 mg of the copper oxide prepared in the previous step were added to a mortar, stirred evenly at 25° C., and the mixture was manually ground for 40 min. The obtained product was washed with deionized water and vacuum dried at 30° C. for 8 h to obtain chlorine-doped copper oxide.
[0134] Embodiment 39
[0135] 100 mg of sodium chloride and 500 mg of commercial copper powder were added to a polytetrafluoroethylene ball mill, followed by 5 mm diameter stainless steel grinding balls and 8 mm diameter stainless steel grinding balls, with a ball-to-material mass ratio of 30:1. The reaction temperature was set to 50 °C, the speed of the ball mill was controlled to 800 rpm, and mechanical grinding was performed in an air atmosphere for 3 hours. During the grinding process, the copper powder reacted with oxygen in the air to generate cuprous oxide, and then halogen doping was achieved by the reaction of cuprous oxide with sodium chloride under grinding conditions. The resulting product was washed with deionized water and vacuum dried at 30 °C for 8 hours to obtain chlorine-doped cuprous oxide.
[0136] Embodiment 40
[0137] 300 mg of commercial cobalt powder was added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 30:1. The reaction temperature was set to 250°C, the speed of the ball mill was controlled to 1000 rpm, and mechanical grinding was performed in an air atmosphere for 15 hours, and oxidation reaction occurred in full contact with air to obtain cobalt oxide.
[0138] 150 mg of sodium bromide and 200 mg of the cobalt oxide prepared in the previous step were added to a polytetrafluoroethylene ball mill, and then 5 mm diameter zirconium oxide grinding balls and 8 mm diameter zirconium oxide grinding balls were added, and the ball-to-material mass ratio was 15:1. The reaction temperature was set to 30 ° C, the ball mill speed was 600 rpm, and mechanical grinding was performed under vacuum for 2 hours. The obtained solid product was washed with deionized water and vacuum dried at 30 ° C for 8 hours to obtain bromine-doped cobalt oxide.
[0139] Embodiment 41
[0140] 500 mg of commercial iron powder was added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material mass ratio of 30:1. The reaction temperature was set to 80°C, the speed of the ball mill was controlled to 800 rpm, and mechanical grinding was performed in an air atmosphere for 24 hours, and oxidation reaction occurred in full contact with air to obtain ferric oxide.
[0141] 36 mg of magnesium chloride and 100 mg of ferric oxide prepared in the previous step were added to a mortar, stirred evenly at 25° C., and the mixture was manually ground for 60 min. The obtained product was washed with deionized water and vacuum dried at 30° C. for 8 h to obtain chlorine-doped ferric oxide.
[0142] Embodiment 42
[0143] 15g of copper chloride, 25g of sodium sulfite and 2mL of formic acid were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5mm and 8mm were added, with a ball-to-material ratio of 15:1. The reaction temperature was set to 40°C, the speed of the ball mill was controlled to 600rpm, and mechanical grinding was performed under a nitrogen atmosphere for 1h. The obtained solid was repeatedly washed with deionized water for more than three times to obtain nano cuprous oxide.
[0144] 300 mg of potassium iodide and 100 mg of nano cuprous oxide were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material ratio of 20:1. The reaction temperature was set to 30°C, the speed of the ball mill was controlled to 600 rpm, and mechanical grinding was performed under nitrogen atmosphere for 30 min. The obtained solid product was washed with deionized water and vacuum dried at 50°C for 7 h to obtain iodine-doped nanoparticles.
[0145] Cuprous oxide.
[0146] Embodiment 43
[0147] 15g of cobalt acetate and 15g of oxalic acid were mixed and ground in a dry mortar. The mixture gradually became a liquid paste. After grinding for 15 minutes, the paste began to solidify. After grinding for 30 minutes, the solid phase reaction was basically completed. The obtained solid product was washed with deionized water, filtered, dried under an infrared lamp, and calcined in a muffle furnace at 350°C for 5 hours to obtain cobalt oxide powder.
[0148] 50 mg of sodium fluoride and 100 mg of cobalt oxide were added to a mortar, stirred evenly at 35° C., and the mixture was manually ground for 30 min. The obtained product was washed with deionized water and vacuum dried at 30° C. for 8 h to obtain fluorine-doped cobalt oxide.
[0149] Embodiment 44
[0150] 30g of copper sulfate pentahydrate, 100g of ascorbic acid and 2mL of formic acid were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5mm and 8mm were added, with a ball-to-material ratio of 20:1. The reaction temperature was set to 40°C, the speed of the ball mill was controlled to 600rpm, and mechanical grinding was performed for 30min under an argon atmosphere. The obtained solid was repeatedly washed with deionized water for more than three times to obtain nano cuprous oxide.
[0151] 150 mg of sodium chloride and 100 mg of nano cuprous oxide were added to a polytetrafluoroethylene ball mill, and then stainless steel grinding balls with a diameter of 5 mm and stainless steel grinding balls with a diameter of 8 mm were added, with a ball-to-material ratio of 20:1. The reaction temperature was set to 30°C, the speed of the ball mill was controlled to 600 rpm, and mechanical grinding was performed under an argon atmosphere for 1 h. The obtained solid product was washed with deionized water and vacuum dried at 50°C for 6 h to obtain chlorine-doped nano cuprous oxide.
[0152] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.
Claims
1. An application of halogen-doped metal oxide nanozyme in peroxidase-like catalysis, characterized in that: The grinding preparation method of the halogen-doped metal oxide nanozyme comprises the following steps: mixing a metal precursor with a halogen precursor at a temperature between 0 and 100° C., manually grinding or ball milling the mixture, washing the obtained product with deionized water, and drying to obtain a halogen-doped metal oxide nanozyme; The peroxidase-like catalytic conditions are to evaluate the performance of the halogen-doped metal oxide nanozyme in catalyzing the activation of hydrogen peroxide and promoting the oxidation of the substrate in a solution in which the substrate 3,3',5,5'-tetramethylbenzidine and hydrogen peroxide are present; The peroxidase-like catalysis is used in antibacterial and dye degradation, wherein the antibacterial application is to evaluate the inhibitory effect of the halogen-doped metal oxide nanozyme on drug-resistant Staphylococcus aureus by counting the number of colonies in an acidic environment through a plate coating method; the dye degradation application is to evaluate the performance of the halogen-doped metal oxide nanozyme in dye degradation by comparing the changes in absorbance of Rhodamine B and methyl orange organic dyes before and after degradation in an acidic environment; The metal precursor is a metal oxide or a metal powder; the halogen precursor is one or a combination of alkali metal halides, alkaline earth metal halides, and ammonium halides; The metal oxide is any one or a combination of several of copper oxide, cuprous oxide, zinc oxide, titanium dioxide, cobalt oxide, cobalt tetroxide, cobalt trioxide, ferric oxide, ferric oxide, cerium dioxide, manganese dioxide, manganese tetroxide, manganese trioxide, aluminum oxide, molybdenum dioxide, molybdenum trioxide, vanadium pentoxide, nickel oxide, magnesium oxide, calcium oxide, barium oxide, tungsten trioxide, zirconium dioxide, ruthenium dioxide, LaNiO3, LaCoO3, LaMnO3, and SrFeO3, and the corresponding metal oxide is a commercial metal oxide or a synthetic metal oxide; the metal powder is any one or a combination of several of copper powder, iron powder, and cobalt powder.
2. The use of a halogen-doped metal oxide nanozyme for peroxidase-like catalysis according to claim 1, characterized in that: The drying is vacuum drying or oven drying, the drying temperature is 30-50° C., and the drying time is 6-8 hours.
3. The use of a halogen-doped metal oxide nanozyme for peroxidase-like catalysis according to claim 1, characterized in that: The molar ratio of the metal in the metal precursor to the halogen ion in the halogen precursor is 1:0.1-8.
4. The use of a halogen-doped metal oxide nanozyme for peroxidase-like catalysis according to claim 1, characterized in that: The manual grinding reaction time is 10 to 60 minutes; the ball milling reaction time is 5 minutes to 12 hours; the manual grinding is to grind the mixture manually in a mortar; the ball milling is to add the mixture and grinding balls into a ball mill jar for mechanical grinding.
5. The use of a halogen-doped metal oxide nanozyme for peroxidase-like catalysis according to claim 1, characterized in that: The ball-to-material mass ratio in the ball milling reaction is 10-30:1; the atmosphere of the ball milling reaction is one of air, nitrogen, argon or vacuum.
6. The use of a halogen-doped metal oxide nanozyme for peroxidase-like catalysis according to claim 4, characterized in that: The grinding balls are zirconia balls or stainless steel balls, the diameter of the grinding balls is 3-40 mm, and the density of the grinding balls is not less than 6 g / cm 3 ; The rotation speed of the ball mill is 600~1000rpm.