Method for synthesizing highly colloid-soluble pseudo-boehmite using carbon dioxide as raw material

By using carbon dioxide as raw material, carbonization method and low-temperature slurry rapid aging method, the problems of high cost and high energy consumption in the synthesis process of phthal-thalthal-water alumina are solved, and the low cost of phthal-thalthal-water alumina is achieved. Low energy consumption preparation, suitable for catalyst synthesis field.

CN115974113BActive Publication Date: 2024-11-15ZHONGKE CATALYSIS NEW TECH (DALIAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211670309.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-11-15
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

The existing synthesis process of phthalid water-thin water-thin synthesis has problems such as raw material toxicity, high post-treatment temperature, long aging time and high cost, and a low-cost and low energy consumption high-performance phthalid water-thin synthesis is urgently needed.

Method used

Carbon dioxide is used as raw material to prepare high-gel solubility pseudo-thin aluminite through carbonization, and low-temperature beating and rapid aging are used to reduce energy consumption and improve production efficiency.

Benefits of technology

It has achieved low-cost and low-energy preparation of high-gum-soluble phthalite, with green and environmentally friendly characteristics, and is suitable for the field of catalyst synthesis, simplifying the process flow and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115974113B_ABST
    Figure CN115974113B_ABST
Patent Text Reader

Abstract

The present invention provides a method for synthesizing highly colloid-soluble pseudo-boehmite using carbon dioxide as a raw material, and belongs to the field of catalyst materials. In the present invention, carbon dioxide is introduced into a pre-configured sodium aluminate solution to react and form a gel, and the obtained slurry is pulped at low temperature, and then rapidly aged to obtain highly colloid-soluble pseudo-boehmite. Since the present invention adopts a carbonization method, pulps at low temperature, and rapidly ages, the reaction raw materials are green and environmentally friendly, low in cost, and energy consumption is reduced, which is conducive to industrial operation. The synthesized pseudo-boehmite has high colloid solubility and complete crystal form, and can be widely used in the field of catalyst synthesis, filling the gap in domestic raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst materials. Technical Background

[0002] Pseudo-boehmite, also known as pseudo-boehmite, boehmite colloid or boehmite-like, is a group of aluminum oxide hydrates with uncertain composition and incomplete crystallization, evolving from disorder to order, weak crystalline to crystalline. Its molecular formula is Al 2 O 3 ·nH 2 O (n = 1.4-2.0). It is widely used because of its large specific surface area and pore volume, high thermal stability and high thixotropic gelation. Among them, the peptization of pseudo-boehmite under acidic conditions as a binder for catalytic cracking, hydrogenation and other catalysts is an important application in the petrochemical industry. Peptized pseudo-boehmite as a binder can increase the mechanical strength and pore structure of the catalyst to a certain extent, improve the catalytic performance of the catalyst, and provide suitable acidity. Therefore, the peptization performance of pseudo-boehmite is directly related to the selectivity, stability and activity of the catalyst.

[0003] At present, the industrialized synthesis processes of pseudo-boehmite are mainly alcohol-aluminum method and carbonization method. Patent CN106629794B discloses a method for synthesizing highly soluble pseudo-boehmite. The pseudo-boehmite prepared by alcohol-aluminum method has the advantages of good peptization performance, concentrated pore distribution, single crystal phase, etc. However, the organic solvent used in alcohol-aluminum method has certain toxicity, high import cost, complex process and difficult to promote. Patent CN110304644B provides a method for preparing high-performance pseudo-boehmite. This method uses cheap Al(OH) 3 As raw material, high-viscosity pseudo-boehmite is synthesized by traditional carbonization method, and its peptization index is as high as over 97%. However, the pulping temperature is 80-100℃, the aging method is high temperature and high pressure, and high carbon alcohol is used as an additional additive, which increases production energy consumption and cost.

[0004] At present, the process of synthesizing highly colloid-soluble pseudo-boehmite has disadvantages such as toxic raw materials, high post-processing temperature, long aging time and high cost. Therefore, there is an urgent need for a low-cost, low-energy consumption, high-performance pseudo-boehmite preparation method. Summary of the invention

[0005] In view of the above, in order to address the shortcomings of the prior art, the present invention provides a method for synthesizing highly soluble pseudo-boehmite using carbon dioxide as a raw material, wherein the pseudo-boehmite colloid obtained by carbonization is pulped and aged at low temperature to quickly obtain highly soluble pseudo-boehmite.

[0006] A method for synthesizing highly peptized pseudo-boehmite using carbon dioxide as a raw material, the method comprising:

[0007] (1) Preparation and purification of pre-prepared solution: Aluminum hydroxide and liquid alkali are reacted to obtain a sodium aluminate pre-prepared solution, which is filtered to obtain a clear and transparent solution;

[0008] (2) Dilution and gelling: The pre-mixed solution is diluted with water and carbon dioxide is introduced to obtain a pseudo-boehmite slurry;

[0009] (3) Centrifugation and low-temperature beating: The slurry is processed by a centrifuge at a speed of 3000-5000 r / min for 2-15 minutes to obtain a pseudo-boehmite wet material, and then the pseudo-boehmite wet material is beaten 3-7 times at 15-25°C with washing water containing an auxiliary agent, and the beating time is 5-15 minutes. Centrifugation is required after each beating;

[0010] (4) Rapid aging: The pulped samples were aged in an oven at 65-95°C for 3-10 h;

[0011] (5) Drying to obtain pseudo-boehmite: After aging, the sample is dried in an oven at 50-80°C for 6-12 hours.

[0012] The caustic ratio of the oxides in the pre-mixed liquid raw material in step (1) is 1.3-2.0.

[0013] The Al in the sodium aluminate solution after dilution in step (2) 2 O 3 The concentration is 20-80g / L.

[0014] The auxiliary agent added to the washing water in step (3) is nitric acid or ammonium chloride, and the amount of the auxiliary agent added is 0.2-1.2wt%.

[0015] In the step (4), the aging method is dynamic or static, and the heating step is one-stage or two-stage.

[0016] The highly colloid-soluble pseudo-boehmite is prepared by any of the methods described above.

[0017] The present invention introduces carbon dioxide into a pre-prepared sodium aluminate pre-mixed liquid to react and form a gel, obtains a slurry, and then beats it at low temperature, and then rapidly ages it to obtain pseudo-boehmite with high gel solubility. Since the present invention adopts a carbonization method, low-temperature beating, rapid aging, green raw materials, low cost, reduced energy consumption, and is conducive to industrial operation. The synthesized pseudo-boehmite has the characteristics of high gel solubility, complete crystal form, high purity, etc., and can be used in the field of catalyst synthesis.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) Compared with other pseudo-boehmite synthesis processes, it takes less time and consumes less energy, which is conducive to industrial production;

[0020] (2) The process of synthesizing pseudo-boehmite is simple and controllable, and the raw materials used are non-toxic and green and environmentally friendly, which meets my country's environmental protection requirements, and the production cost is low;

[0021] (3) The synthesized pseudo-boehmite has high colloidal solubility, complete crystal form and high purity, and can be directly used as a raw material for molecular sieve synthesis and a catalyst carrier. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the XRD spectrum of the product in Example 1. DETAILED DESCRIPTION

[0023] The present invention provides a method for measuring the peptization index of pseudo-boehmite, and the specific operation is as follows:

[0024] (1) The pseudo-boehmite is subjected to thermogravimetric test. The solid residual mass percentage of the thermogravimetric result at 800°C*2g is the solid content of the pseudo-boehmite, recorded as M0;

[0025] (2) Weigh (1.4 / M0) g of sample into a beaker, add (M0*10-1.4 / M0) g of water, and dilute the reagent to contain 10% Al 2 O 3 slurry, add (M0*0.2 / 1.4) g nitric acid under stirring, continue stirring for 10 min to obtain a clear solution;

[0026] (3) Weigh about 6 g of the solution obtained in step (2) into a test tube, centrifuge (4000 r / min, 15 min), pour the supernatant in the test tube into a crucible, dry it in an oven at 120° C. for 1 h, then transfer it to a muffle furnace and heat it to 550° C. at 10° C. / min for 1 h, cool it, and record the mass of the dried solid in the crucible as W1;

[0027] (4) Weigh the same mass of the clarified solution as in step (3) into a crucible, dry it in an oven at 120° C. for 1 h, then transfer it to a muffle furnace and heat it to 550° C. at a rate of 10° C. / min for 1 h, cool it, and record the mass of the dried solid in the crucible as W2;

[0028] (5) Calculation results: Peptization index = W1 / W2*100%.

[0029] The present invention is described in detail below by way of examples, but the present invention is not limited to these examples.

[0030] Example 1

[0031] Preparation of pre-mixed solution: First, add 259g of liquid alkali into a beaker, add 125g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle to react to obtain a sodium aluminate solution, and finally filter it to obtain a clear and transparent solution. The caustic ratio of the oxide in the raw material is 1.3.

[0032] Preparation of highly colloid-soluble pseudo-boehmite: First, take the above-prepared solution and dilute it with water until Al 2 O 3 The concentration is 60g / L, and carbon dioxide is introduced into the mixture to form a gel to obtain a pseudo-boehmite slurry. The slurry is then centrifuged at 4000r / min for 5 minutes in a centrifuge to obtain a pseudo-boehmite wet material. The wet material is then pulped 5 times in a 1wt% nitric acid aqueous solution at 25°C, and pulped once with distilled water. Each pulping lasts for 5 minutes, and centrifugation is required after each pulping. The wet material is heated to 95°C in a drying oven in one step, dynamically aged for 10 hours, and finally the aged sample is dried at 65°C for 8 hours to obtain a highly colloid-soluble pseudo-boehmite. The XRD spectrum is shown in Figure 1 shown.

[0033] Example 2

[0034] Preparation of pre-mixed solution: First, add 430g of liquid alkali into a beaker, add 151g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle to react to obtain a sodium aluminate solution, and finally filter it to obtain a clear and transparent solution. The caustic ratio of the oxide in the raw material is 1.8.

[0035] Preparation of highly colloid-soluble pseudo-boehmite: First, take the above-prepared solution and dilute it with water until Al 2 O 3 The concentration is 26g / L, and carbon dioxide is introduced into the gel to obtain pseudo-boehmite slurry. The slurry is then centrifuged at 4500r / min for 3 minutes in a centrifuge to obtain pseudo-boehmite wet material. The wet material is then pulped 3 times in a 0.2wt% nitric acid aqueous solution at 23°C, and pulped once with distilled water, each time for 15 minutes, and centrifuged after each pulping. The wet material is heated to 95°C in a drying oven in one step, statically aged for 4 hours, and finally the aged sample is dried at 65°C for 6 hours to obtain highly colloid-soluble pseudo-boehmite.

[0036] Example 3

[0037] Preparation of pre-mixed solution: First, add 78g of liquid alkali into a beaker, add 38g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle for reaction to obtain a sodium aluminate solution, and finally filter it to obtain a clear and transparent solution. The caustic ratio of the oxide in the raw material is 1.3.

[0038] Preparation of highly colloid-soluble pseudo-boehmite: First, take the above-prepared solution and dilute it with water until Al 2 O 3 The concentration is 28g / L, and carbon dioxide is introduced into the gel to obtain pseudo-boehmite slurry. The slurry is then centrifuged at 3000r / min for 15min in a centrifuge to obtain pseudo-boehmite wet material. The wet material is then pulped twice in 0.2wt% ammonium chloride solution at 15°C, and pulped twice with distilled water, each time for 15min, and centrifuged after each pulping. The wet material is heated in two stages in an oven, the first stage is heated to 70°C, static aging for 1h, the first stage is heated to 95°C, static aging for 6h, and finally the aged sample is dried at 80°C for 5h to obtain highly colloid-soluble pseudo-boehmite.

[0039] Example 4

[0040] Preparation of pre-mixed solution: First, add 129g of liquid alkali into a beaker, add 62g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle to react to obtain a sodium aluminate solution, and finally filter it to obtain a clear and transparent solution. The caustic ratio of the oxide in the raw material is 1.3.

[0041] Preparation of highly colloid-soluble pseudo-boehmite: First, take the above-prepared solution and dilute it with water until Al 2 O 3 The concentration is 42g / L, and carbon dioxide is introduced into the gel to obtain pseudo-boehmite slurry. The slurry is then centrifuged at 3500r / min for 12 minutes to obtain pseudo-boehmite wet material. The wet material is then pulped 5 times in 0.6wt% nitric acid solution at 20°C, pulped once with distilled water, and each pulping lasts 10 minutes. Centrifugation is required after each pulping. The wet material is heated to 95°C in a drying oven in one step, dynamically aged for 5 hours, and finally the aged sample is dried at 70°C for 8 hours to obtain highly colloid-soluble pseudo-boehmite.

[0042] Example 5

[0043] Preparation of pre-mixed solution: First, add 215g of liquid alkali into a beaker, add 104g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle to react to obtain a sodium aluminate solution, and finally filter it to obtain a clear and transparent solution. The caustic ratio of the oxide in the raw material is 1.3.

[0044] Preparation of highly colloid-soluble pseudo-boehmite: First, take the above-prepared solution and dilute it with water until Al 2 O 3The concentration is 42g / L, and carbon dioxide is introduced into the mixture to form a gel to obtain a pseudo-boehmite slurry. The slurry is then centrifuged at 4300r / min for 5 minutes in a centrifuge to obtain a pseudo-boehmite wet material. The wet material is then pulped 6 times in a 0.4wt% nitric acid solution at 23°C, and pulped once with distilled water, each time for 10 minutes, and centrifuged after each pulping. The wet material is heated to 95°C in a drying oven in one step, dynamically aged for 5 hours, and finally the aged sample is dried at 65°C for 10 hours to obtain a highly colloid-soluble pseudo-boehmite.

[0045] Example 6

[0046] Preparation of pre-mixed solution: First, add 215g of liquid alkali into a beaker, add 104g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle to react to obtain a sodium aluminate solution, and finally filter it to obtain a clear and transparent solution. The caustic ratio of the oxide in the raw material is 1.3.

[0047] Preparation of highly colloid-soluble pseudo-boehmite: First, take the above-prepared solution and dilute it with water until Al 2 O 3 The concentration is 43g / L, and carbon dioxide is introduced into the mixture to form a gel to obtain a pseudo-boehmite slurry. The slurry is then centrifuged at 4300r / min for 5 minutes in a centrifuge to obtain a pseudo-boehmite wet material. The wet material is then pulped 3 times in a 0.5wt% nitric acid solution at 23°C, and pulped once with distilled water, each time for 7 minutes, and centrifuged after each pulping. The wet material is heated to 95°C in a drying oven in one step, statically aged for 10 hours, and finally the aged sample is dried at 65°C for 7 hours to obtain a highly colloid-soluble pseudo-boehmite.

[0048] Example 7

[0049] Preparation of pre-mixed solution: First, add 433g of liquid alkali into a beaker, add 209g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle to react to obtain a sodium aluminate solution, and finally filter it to obtain a clear and transparent solution. The caustic ratio of the oxide in the raw material is 1.4.

[0050] Preparation of highly colloid-soluble pseudo-boehmite: First, take the above-prepared solution and dilute it with water until Al 2 O 3The concentration is 80g / L, and carbon dioxide is introduced into the mixture to form a gel to obtain a pseudo-boehmite slurry. The slurry is then centrifuged at 4200r / min for 3 minutes in a centrifuge to obtain a pseudo-boehmite wet material. The wet material is then pulped 4 times in a 1wt% nitric acid solution at 23°C, and pulped twice with distilled water, each time for 15 minutes, and centrifuged after each pulping. The wet material is heated to 95°C in a drying oven in one step, dynamically aged for 10 hours, and finally the aged sample is dried at 65°C for 10 hours to obtain a highly colloid-soluble pseudo-boehmite.

[0051] The parameters of the highly soluble pseudo-boehmite synthesized using carbon dioxide as raw material are shown in Table 1.

[0052] Table 1 Parameters of high-colloid pseudo-boehmite

[0053]

[0054] Note 1: The peptization index is obtained by the peptization test method introduced above; Note 2: The relative crystallinity is the percentage of the sum of the peak heights of the three main peaks in the XRD characterization results of the example sample to the standard sample.

[0055] The present invention is described by way of embodiments, and those skilled in the art will appreciate that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application belong to the protection scope of the present invention.

Claims

1. A method for synthesizing highly colloid-soluble pseudo-boehmite using carbon dioxide as a raw material, characterized in that: The method is: Preparation of pre-mixed liquid: first, add 259g of liquid alkali into a beaker, add 125g of aluminum hydroxide in batches while stirring, continue stirring for a period of time, then transfer to a crystallization kettle for reaction to obtain a sodium aluminate solution, and finally filter the sodium aluminate solution to obtain a clear and transparent solution, wherein the caustic ratio of the oxide in the pre-mixed liquid raw material is 1.3; Preparation of highly colloid-soluble pseudo-boehmite: first, take the pre-prepared liquid obtained above and dilute it with water until the Al2O3 concentration in the solution is 60g / L, and introduce carbon dioxide to form a gel to obtain a pseudo-boehmite slurry. Subsequently, the slurry is centrifuged at 4000r / min for 5 minutes in a centrifuge to obtain a pseudo-boehmite wet material. Then, the wet material is pulped 5 times at 25°C using a 1wt% nitric acid aqueous solution and pulped once with distilled water, each time for 5 minutes. Centrifugation is required after each pulping. The obtained wet material is heated to 95°C in an oven in one step, dynamically aged for 10 hours, and finally the aged sample is dried at 65°C for 8 hours to obtain a highly colloid-soluble pseudo-boehmite.