Nano-MgO particles regulating ultrafine-grained magnesium-based composite materials and processing methods thereof

Through low-temperature slow extrusion process and nano-MgO particle regulation, ultrafine crystal magnesium-based composite materials are formed, which solves the problems of taking into account both mechanical properties and corrosion resistance of magnesium alloys, and achieves the effects of high strength, high corrosion resistance and low alloying. , simplifies the preparation process and is suitable for large-scale production.

CN115976383BActive Publication Date: 2024-11-22TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210185264.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-28
Publication Date
2024-11-22
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

It is difficult to take into account the mechanical properties and corrosion resistance of existing magnesium alloys, especially under low alloying conditions, to achieve high yield strength and appropriate degradation rates at the same time. Moreover, the preparation process of existing ultrafine crystal magnesium alloys is complex and difficult to large. Large-scale production.

Method used

Low-temperature slow extrusion process and nano-MgO particle regulation are adopted to form ultrafine crystal structures through dynamic recrystallization, reducing the content of alloy elements except magnesium, and achieving high-strength, high corrosion resistance, and low alloying magnesium-based composite materials.

Benefits of technology

It significantly improves the mechanical properties and corrosion resistance of the material, achieves high yield strength and elongation under low alloying conditions, simplifies the preparation process, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976383B_ABST
    Figure CN115976383B_ABST
Patent Text Reader

Abstract

The invention discloses a nano-MgO particle-regulated ultrafine-grained magnesium-based composite material and a processing method thereof, the processing method comprising the following steps: keeping the cast magnesium-based composite material at a first preset temperature for at least 4 hours, cooling it in warm water, and obtaining a solid-solution magnesium-based composite material; hot-extruding the solid-solution magnesium-based composite material, cooling it at room temperature, and obtaining a nano-MgO particle-regulated ultrafine-grained magnesium-based composite material, wherein the temperature of the hot extrusion is 150-400°C, and the extrusion rate of the hot extrusion is 0.01-1.0 mm / s. The proportion of recrystallized grains in the nano-MgO particle-regulated ultrafine-grained magnesium-based composite material of the invention should be greater than 75%, the average grain size should be less than 1 μm, the mechanical properties should be greater than 376 MPa, and the average annual corrosion rate measured after 28 days of standard immersion experiment using SBF solution according to ASTM G31-72 standard should not be higher than 0.81 mm / y.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of magnesium alloy manufacturing, and in particular relates to an ultrafine-grained magnesium-based composite material controlled by nano-MgO particles and a processing method thereof. Background Art

[0002] Medical magnesium alloys, with their significantly superior mechanical properties compared to biodegradable polymers and ceramics, excellent biocompatibility, and unique corrosion absorption properties, have become a representative example of a new generation of high-strength, low-modulus, biodegradable implant materials. They hold enormous market potential in clinical applications such as fracture fixation, interventional treatments with vascular and luminal stents, surgical staplers, and closure clips. Since 2005, researchers in China and abroad have enhanced the strength and corrosion resistance of magnesium and its alloys through alloying, surface coatings, and ceramic particle-reinforced composites. After more than a decade of basic research and in vitro and in vivo implantation experiments, commercialized biodegradable magnesium alloy vascular stents and bone screws have been developed in Germany, Japan, and South Korea, demonstrating excellent safety and efficacy in clinical applications. Related products developed by some domestic researchers and research institutions are still undergoing product approval or third-party evaluation. However, this does not mean that biodegradable magnesium alloys have fully met the requirements for clinical use. For fracture fixation alone, medical magnesium alloys do not yet meet the clinical requirements of yield strength greater than 300 MPa, elongation greater than 10%, and degradation rate less than 0.5 mm / y. Although surface coating technology can control the corrosion degradation rate of magnesium alloys, under complex stresses, the surface coating of bone screws is prone to cracking, which can cause pitting or crevice corrosion, accelerating the degradation of magnesium. Therefore, from the perspective of long-term service, improving the corrosion resistance of magnesium alloy implants is the primary condition for promoting magnesium materials as bone fixation materials. Therefore, the development of fully degradable magnesium alloys with both high yield strength and a suitable degradation rate is of great significance.

[0003] Generally speaking, increasing the content of alloying elements other than magnesium in magnesium alloys is one of the main ways to improve their mechanical properties. However, for biomedical degradable magnesium alloys, the selection of alloying elements other than magnesium must ensure their biosafety and biocompatibility. At the same time, the content of each element in the magnesium alloy should also be reasonably controlled. Although increasing the content of alloying elements other than magnesium will improve the mechanical properties of the material, the large amount of second phases brought about by increasing the content of alloying elements other than magnesium will weaken the corrosion resistance of the material. This is obviously inconsistent with the design concept of high-strength and high-corrosion-resistant alloys. Therefore, the use of low-alloying methods to reduce the content of alloying elements other than magnesium can effectively reduce the negative impact of the second phase on the corrosion resistance of the alloy. However, the reduction of alloying elements other than magnesium often significantly reduces the mechanical properties of the material.

[0004] Existing research (Scripta Mater 2010;63:1024, Materials Science and Engineering:A 2016;677:367, Materials Science and Engineering:A 2013;576:6) indicates that the content of alloying elements other than magnesium in extruded Mg-Zn-Ca alloys is positively correlated with the mechanical properties of the material. Specifically, mechanical properties improve with increasing content of alloying elements other than magnesium. The mechanical properties of these alloys are shown in Table 1 below. As can be seen from the data in Table 1, the mechanical properties of the material increase with increasing content of alloying elements other than magnesium. Mg-Zn-Ca alloys with low content of alloying elements other than magnesium struggle to achieve high mechanical properties. Therefore, improving the mechanical properties of the material while maintaining low alloying content has become an urgent issue.

[0005]

[0006] Nano-MgO particles have been shown to exhibit excellent interfacial bonding with magnesium alloy matrices (Mater Charact 2018; 144:120). Furthermore, the addition of nano-MgO particles can inhibit grain boundary migration and grain growth during hot extrusion, thereby helping the material achieve a finer grain size (Metals-Basel 2020; 10:1357). However, to date, conventional processing methods have limited the grain size of MgO / Mg-Zn-Ca composites to >1.5 μm (Mater Charact 2018; 144:120). According to the classic Hall-Petch relationship for mechanical properties, grain refinement can significantly improve the mechanical properties of metal materials. In particular, when the grain size is refined to the ultrafine grain range (d < 1 μm), the material's strength can be significantly enhanced. At the same time, studies have shown that there is a Hall-Petch relationship between the grain size and corrosion resistance of magnesium alloys, that is, grain refinement can improve the corrosion resistance of the material (Scripta Mater 2010; 63:1201).

[0007] Clearly, further refining the grain size of composite materials based on existing processes can further improve their performance. However, magnesium alloys have low melting points and are difficult to deform. Existing technologies for preparing ultrafine-grained magnesium alloys rely primarily on methods involving severe plastic deformation, such as high-pressure torsion, equal channel angular pressing, and extrusion deformation. Generally speaking, when the content of alloying elements other than magnesium in magnesium alloys is high, a large amount of intermetallic compounds tends to form in the alloy matrix. These intermetallic compounds inhibit grain boundary migration during extrusion and promote the formation of an ultrafine-grained structure. However, this effect does not hold true when the content of alloying elements other than magnesium is low. Furthermore, the temperature and speed during extrusion also play a role in the formation of an ultrafine-grained structure. From a thermodynamic perspective, dynamic recrystallization requires external energy, and increasing the heating temperature promotes dynamic recrystallization to a certain extent. However, higher temperatures cause the grains that have undergone dynamic recrystallization to grow, preventing the formation of an ultrafine-grained structure. Lower temperatures, while suppressing the temperature-induced grain growth, also inhibit the dynamic recrystallization process.

[0008] For example, patent application number CN201210516981.6, entitled “A high-yield processing method for ultrafine-grained magnesium alloy sheets,” discloses a method for obtaining ultrafine-grained magnesium alloy sheets by rolling after isochannel extrusion of magnesium alloys. Patent application number 201610589439.1, entitled “A method for preparing bulk nanocrystalline magnesium alloys with small deformation,” discloses a method for preparing nanocrystalline (40-100nm) Mg-Ag alloys using room temperature cold rolling deformation and subsequent low-temperature short-time heat treatment. However, these two processes are complex in preparation and require multiple deformation passes to achieve the preparation of ultrafine-grained materials. This process is difficult to apply to large-scale production, and the elongation and strength of the resulting materials cannot meet the engineering requirements for matching material strength and elongation. Patent application number 202010873447.5, entitled "An ultrafine-grained deformable magnesium alloy material and its preparation method", discloses a patent for preparing an ultrafine-grained high rare earth content (the mass ratio of all alloy elements except magnesium is greater than 13%) magnesium alloy by a simple reverse extrusion method. The average grain size given in the embodiment is 5-6μm, which is not the ultrafine-grained structure widely recognized internationally (d<1μm). At the same time, the content of alloy elements other than magnesium is relatively high.

[0009] Figure 1 The content of alloying elements other than magnesium, the corresponding yield strength and elongation of representative Mg-Zn(Ca) based alloys and composites are summarized. Figure 1It is not difficult to see that materials with ultrafine grain structure, such as hot extruded ultrafine grained magnesium (Mg-2Zn-0.7Ca-1Mn alloy, J.Magnes.Alloy., 2021, 9(4), 1428-1442 and Mg-4Zn-0.5Ca-0.5Tic composite material, T Nonferr Metal Soc, 2020, 30(9), 2394-2412), ultrafine grained magnesium prepared by equal channel method (Mg-0.6Zn-0.6Ca alloy, Mater.Sci.Eng.A, 2021, 826, 142002) and ultrafine grained magnesium prepared by high pressure torsion (Mg-6.2Zn-0.5Zr-0.2Ca alloy, Scripta Materialia, 2017, 131, 1-5), often have better properties than hot extruded non-ultrafine grained magnesium (Mg-3Zn-0.2Ca-0.5MgO composite material, Mater [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] [The following sentences appear unrelated and likely represent fragments of unrelated text.] Summary of the Invention

[0010] In response to the shortcomings of the existing technology, the purpose of the present invention is to provide a processing method for regulating ultrafine-grained magnesium-based composite materials using nano-MgO particles. Based on the technical solution of Patent No. ZL201610307112.0 (self-protected degradable MgO / Mg-Zn-Ca biocomposite materials), this processing method reduces the content of alloying elements other than magnesium and uses a low-temperature slow extrusion method to achieve a short process that can continuously and mass-produce a low-alloyed magnesium-based composite material (MgO / Mg-Zn-Ca) with an ultrafine-grained structure, high strength and toughness, high corrosion resistance.

[0011] The purpose of the present invention is achieved through the following technical solutions.

[0012] A method for processing an ultrafine-grained magnesium-based composite material regulated by nano-MgO particles comprises the following steps:

[0013] S1: obtaining a cast magnesium-based composite material, wherein the cast magnesium-based composite material is composed of 0.5-1wt% of Zn, 0.2-0.5wt% of Ca, 0.5-1.5wt% of MgO, and the balance of Mg, and the total weight of MgO, Zn, and Ca is 1.5-2.5wt% of the cast magnesium-based composite material;

[0014] In the S1, the cast magnesium-based composite material consists of 0.8-1 wt% of Zn, 0.2 wt% of Ca, 1-1.5 wt% of MgO and the balance of Mg, calculated by mass percentage.

[0015] In S1, the MgO is nano-MgO particles, and the average diameter of the nano-MgO particles is less than 100 nm.

[0016] S2: keeping the cast magnesium-based composite material at a first preset temperature for at least 4 hours, and placing it in warm water for cooling to obtain a solid solution magnesium-based composite material;

[0017] In the step S2, the first preset temperature is 350-550°C.

[0018] In S2, the first preset temperature holding time is 4 to 36 hours.

[0019] In the step S2, the temperature of the warm water is 60-70°C.

[0020] S3: hot-extrude the solid solution magnesium-based composite material and cool it to room temperature to obtain an ultrafine-grained magnesium-based composite material regulated by nano-MgO particles, wherein the hot extrusion temperature is 150-400° C. and the hot extrusion rate is 0.01-1.0 mm / s.

[0021] In the step S3 , the extrusion ratio of the hot extrusion is (10-60):1.

[0022] In the step S3 , the extrusion rate of the hot extrusion is 0.01 to 0.1 mm / s.

[0023] The nano-MgO particles obtained by the above processing method regulate the ultrafine-grained magnesium-based composite material.

[0024] In the above technical solution, the nano-MgO particles regulate the grain size d of the ultrafine-grained magnesium-based composite material to be: 100nm<d<1μm.

[0025] The processing method of the present invention uses low-temperature, slow extrusion to prepare nano-MgO particles-controlled ultrafine-grained magnesium-based composite materials. The low extrusion temperature and nano-MgO particles can promote the dynamic recrystallization process of the solid-solution magnesium-based composite materials during the extrusion process, so that the solid-solution magnesium-based composite materials produce an ultrafine-grained structure (grain size d < 1 μm) during the extrusion process, thereby obtaining a nano-MgO particle-controlled ultrafine-grained magnesium-based composite material with an ultrafine-grained structure. This significantly improves the mechanical properties of the material. Compared with Comparative Example 1, Example 2 increases the yield strength by approximately 186%, from 152 MPa to 435 MPa, with the same composition. Compared with Comparative Example 3, the yield strength of Example 2 also increases by approximately 34%, from 325 MPa to 435 MPa. This makes it possible to prepare nano-MgO particle-controlled ultrafine-grained magnesium-based composite materials with an ultrafine-grained structure by a one-step extrusion method, greatly improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The nano-MgO particles of the present invention regulate the yield strength and elongation corresponding to the ultrafine-grained magnesium-based composite material and the existing reported Mg-Zn (Ca)-based alloys and composite materials;

[0027] Figure 2 (a, b) SEM, (c) room temperature tensile curve, and (d) corrosion rate of the ultrafine-grained magnesium-based composite material regulated by nano-MgO particles obtained in Example 1;

[0028] Figure 3 (a, b) SEM, (c) room temperature tensile curve, and (d) corrosion rate of the ultrafine-grained magnesium-based composite material regulated by nano-MgO particles obtained in Example 2;

[0029] Figure 4 SEM (a, b) and room temperature tensile curve (c), (d) corrosion rate of the low alloyed magnesium-based composite material prepared by high temperature rapid extrusion obtained in Comparative Example 1;

[0030] Figure 5 (a, b) SEM, (c) room temperature tensile curve, and (d) corrosion rate of the magnesium alloy material with high content of alloying elements other than magnesium obtained in Comparative Example 2;

[0031] Figure 6 The morphology of the nano-MgO particles used in Examples 1 and 2. DETAILED DESCRIPTION

[0032] Pure magnesium (99.99wt.%) Shanxi Yinguang Magnesium Industry

[0033] Pure zinc particles (99.99wt.%) Tianjin Guangfu Chemical

[0034] 70wt.%Mg-30wt.%Ca Master Alloy Shanxi Yinguang Magnesium Industry

[0035] 75wt.%Mg-25wt.%Ca Master Alloy Shanxi Yinguang Magnesium Industry

[0036] The preparation method of nano-MgO particles can be found in 2.1.1 of Preparation and in vitro degradation behavior of biomedical Mg-Zn-Ca-xMgO composite materials and their coatings [D]. Tianjin University of Technology, 2020. DOI: 10.27360 / d.cnki.gtlgy.2020.000363. The diameter of nano-MgO particles is about 35-75nm, and the morphology is as follows. Figure 6 shown.

[0037] The technical solution of the present invention is further described below with reference to specific embodiments.

[0038] A mixed atmosphere of sulfur hexafluoride and nitrogen at a volume ratio of 1:100: 99.99 wt.% nitrogen and 99.99 wt.% sulfur hexafluoride at a volume ratio of 100:1 was used. (Nitrogen: Tianjin Huanyu Gas, sulfur hexafluoride: Tianjin Saimet Gas).

[0039] The cast magnesium-based composite material used in Examples 1 and 2 consists of 1wt% Zn, 0.2wt% Ca, 1wt% MgO, and the balance Mg, in terms of mass percentage. The preparation method is as follows: purchased pure magnesium (99.99wt.%), pure zinc (99.99wt.%), and a 75wt% Mg-25wt% Ca master alloy are melted at 780°C in a magnesium alloy box-type atmosphere furnace with high shear stirring and ultrasonic treatment, and then nano-MgO particles are added. The mixture is treated for 15 minutes under shear stirring at 3500 rpm and 10KHz ultrasonic conditions in a mixed atmosphere of sulfur hexafluoride and nitrogen in a volume ratio of 1:100, and then cast to obtain a cast magnesium-based composite material.

[0040] Average annual corrosion rate: The test is conducted using SBF solution. The sample to be tested is immersed in the SBF solution. The weight loss value of the sample is obtained at different times. The average annual corrosion rate is obtained according to the ASTM G31-72 standard.

[0041] Method for obtaining SBF solution: The required drugs are shown in Table 2 (all reagents are AR analytical grade). The drugs in Table 2 are added to 1 L of distilled water in sequence, and hydrochloric acid (HCl, AR 36%-38%, Shanghai test) is used to adjust the solution pH to 7.4 at 37°C.

[0042] Table 2 Content of ingredients in 1L SBF solution (unit: g)

[0043] NaCl <![CDATA[NaHCO3]]> KCl <![CDATA[NaHPO4·7H2O]]> <![CDATA[MgCl2·6H2O]]> <![CDATA[CaCl2]]> <![CDATA[Na2SO4]]> <![CDATA[(CH2OH)5CNH2]]> 6.5453 2.2683 0.3728 0.2681 0.3050 0.2780 0.0711 6.057

[0044] Example 1

[0045] A method for processing an ultrafine-grained magnesium-based composite material regulated by nano-MgO particles comprises the following steps:

[0046] S1: Obtaining cast magnesium-based composites;

[0047] S2: In a box-type resistance furnace, the cast magnesium-based composite material is kept at a first preset temperature for 16 hours, and then placed in warm water at 60° C. and rapidly cooled to obtain a solid solution magnesium-based composite material, wherein the first preset temperature is 420° C.;

[0048] S3: The solid solution magnesium-based composite material is processed into a rod with a diameter of 60 mm, the solid solution magnesium-based composite material is hot-extruded using a horizontal extruder, and naturally cooled in air at room temperature of 20-25°C to obtain an ultrafine-grained magnesium-based composite material regulated by nano-MgO particles, wherein the hot extrusion temperature is 270°C, the hot extrusion rate is 0.1 mm / s, and the hot extrusion ratio is 56:1.

[0049] Figure 2 The microstructure (a, b), mechanical properties (c), and corrosion resistance (d) of the ultrafine-grained magnesium-based composite material obtained in Example 1, regulated by nano-MgO particles, were statistically measured to have an average grain size of 0.7 μm, a room-temperature tensile yield strength of 377 MPa, an elongation of 10.1%, and an average annual corrosion rate of 0.81 mm / y after 28 days, demonstrating excellent mechanical properties and corrosion resistance.

[0050] The nano-MgO particles obtained in Example 1 control the proportion of recrystallized grains in the ultrafine-grained magnesium-based composite material to be 82%.

[0051] Example 2

[0052] A method for processing an ultrafine-grained magnesium-based composite material regulated by nano-MgO particles comprises the following steps:

[0053] S1: Obtaining cast magnesium-based composites;

[0054] S2: In a box-type resistance furnace, the cast magnesium-based composite material is kept at a first preset temperature for 16 hours, and then placed in warm water at 60° C. and rapidly cooled to obtain a solid solution magnesium-based composite material, wherein the first preset temperature is 420° C.;

[0055] S3: The solid solution magnesium-based composite material is processed into a rod with a diameter of 60 mm, the solid solution magnesium-based composite material is hot-extruded using a horizontal extruder, and naturally cooled in air at room temperature of 20-25°C to obtain an ultrafine-grained magnesium-based composite material regulated by nano-MgO particles, wherein the hot extrusion temperature is 260°C, the hot extrusion rate is 0.01 mm / s, and the hot extrusion ratio is 56:1.

[0056] Figure 3 The nano-MgO particles obtained in Example 2 were used to control the microstructure, mechanical properties, and corrosion resistance of the ultrafine-grained magnesium-based composite material. Statistical measurements showed that even with further reductions in the extrusion temperature, the extruded material still maintained a high degree of complete recrystallization, with an average grain size of 0.46 μm. Its room-temperature tensile yield strength was further increased to 435 MPa, and its elongation was 5.5%. After 28 days, the average annual corrosion rate was 0.68 mm / y, demonstrating excellent mechanical properties and corrosion resistance.

[0057] The nano-MgO particles obtained in Example 2 control the proportion of recrystallized grains in the ultrafine-grained magnesium-based composite material to be 76%.

[0058] Compared with the Mg-Zn (Ca)-based alloys and composite materials reported previously, Example 1 of the present invention can achieve one-step processing of a magnesium-based composite material with an ultrafine grain structure, extremely high mechanical properties and excellent elongation while having a lower content of alloy elements other than magnesium; Example 2, based on Example 1, further enhances the yield strength of the material, bringing the yield strength to 435 MPa.

[0059] Comparative Example 1

[0060] A method for preparing a low-alloyed magnesium-based composite material by high-temperature rapid extrusion is basically the same as the processing method of Example 1, except that the hot extrusion temperature in S3 of Comparative Example 1 is 330°C and the extrusion rate of the hot extrusion is 1 mm / s.

[0061] Figure 4 The microstructure, mechanical properties, and corrosion resistance of the low-alloyed magnesium-based composite material from Comparative Example 1 are shown. The results show that, while maintaining the existing alloy composition (same as in Example 1), higher hot extrusion temperatures and faster extrusion rates significantly impact the material's performance. Statistical measurements show an average grain size of 7 μm, while its room-temperature tensile yield strength is only 152 MPa. Elongation, influenced by grain size, increases to 17.8%.

[0062] Comparative Example 2 (without ceramic particles)

[0063] A method for preparing a magnesium alloy material with a high alloying element content comprises the following steps:

[0064] S1: Obtain a cast magnesium-based composite material, which is composed of 3wt% Zn, 0.2wt% Ca and the remainder Mg in mass percentage; its preparation method is: purchased pure magnesium (99.99wt.%), pure zinc (99.99wt.%) and 75wt% Mg-25wt% Ca intermediate alloy are melted at 720°C in a magnesium alloy box-type atmosphere furnace with high shear stirring and ultrasonic treatment, and treated at 720°C in a mixed atmosphere of sulfur hexafluoride and nitrogen in a volume ratio of 1:100 under shear stirring at 3500 rpm and 10KHz ultrasound for 15 minutes, and cast to obtain a cast magnesium-based composite material.

[0065] S2: In a box-type resistance furnace, the cast magnesium-based composite material is kept at a first preset temperature for 24 hours, and then placed in warm water at 60° C. for rapid cooling to obtain a solid solution magnesium-based composite material, wherein the first preset temperature is 400° C.;

[0066] S3: The solid solution magnesium-based composite material is processed into a rod with a diameter of 60 mm, the solid solution magnesium-based composite material is hot-extruded using a horizontal extruder, and naturally cooled in air at room temperature of 20-25°C to obtain a magnesium alloy material with a high alloy element content, wherein the hot extrusion temperature is 300°C, the hot extrusion rate is 0.5 mm / s, and the hot extrusion ratio is 56:1.

[0067] Figure 5 The microstructure, mechanical properties, and corrosion resistance of the high-alloying element magnesium alloy obtained in Comparative Example 2 are shown. The results show that, even with a high content of alloying elements other than magnesium, low-temperature, slow extrusion can produce an extruded magnesium alloy with an ultrafine grain structure without the addition of ceramic particles. Statistically measured, the average grain size is 4 μm. Without the strengthening effect of the ultrafine grain structure on material properties, the room temperature tensile yield strength is only 236 MPa, and the average annual corrosion rate after 28 days is 1.85 mm / y. The mechanical properties and corrosion resistance exhibited are significantly reduced compared to Examples 1 and 2.

[0068] The alloy composition of the magnesium-based composite material in Comparative Example 1 is the same as that in Example 1, but due to the high temperature of hot extrusion and the fast extrusion rate, the grain size of the low-alloyed magnesium-based composite material is seriously grown, and the mechanical properties are far lower than those of Comparative Example 1 with the same composition material.

[0069] The content of alloying elements other than magnesium in Comparative Example 2 is higher than that of the cast magnesium-based composite materials in Examples 1 and 2. However, due to the lack of the effect of nano-MgO particles, the grain structure of the magnesium alloy obtained in Comparative Example 2 is coarse. Even with a higher content of alloying elements other than magnesium, its mechanical properties are still lower than those of the ultrafine-grained magnesium-based composite material regulated by nano-MgO particles with the addition of nano-MgO particles.

[0070] Comparative Example 3

[0071] The preparation method of the self-protective degradable MgO / Mg-Zn-Ca biocomposite material (patent number: ZL201610307112.0) comprises the following steps:

[0072] Step 1: Alloy Melting

[0073] The invention uses 99.99% pure Mg blocks (Shanxi Yinguang Magnesium Industry), 99.99% pure Zn particles (Tianjin Guangfu), and a 70wt% Mg-30wt% Ca master alloy (Shanxi Yinguang Magnesium Industry) as raw materials, and MgO nanoparticles as reinforcement. The MgO nanoparticles are 60 nm in size. The Mg blocks, Zn particles, 70wt% Mg-30wt% Ca master alloy, and MgO nanoparticles are mixed in a graphite crucible in a mass ratio of 0.3wt% MgO, 3wt% Zn, 0.2wt% Ca, and the balance Mg. The mixture is smelted at 720°C under a gas mixture of 99.6% N2 and 0.4% SF6 by volume for protection. After the alloy is melted, it is stirred thoroughly at 3000 rpm for 12 minutes using a powerful melt stirring paddle. The mixture is then cooled to 680°C and cast into a 60mm diameter composite ingot.

[0074] Step 2: Solution Treatment

[0075] The composite material ingots were subjected to a two-step solution treatment process, with temperatures of 350°C and 510°C for 40 h and 3 h, respectively.

[0076] Step 3: Hot extrusion treatment

[0077] The composite material ingot after solid solution is extruded and deformed at 350° C. The ingot is extruded into a φ6 mm rod, which is a self-protected and degradable MgO / Mg-Zn-Ca biocomposite material.

[0078] The tensile yield strength of the self-protected, biodegradable MgO / Mg-Zn-Ca biocomposite obtained in Comparative Example 3 was 325 MPa. This was also significantly lower than the ultrafine-grained magnesium-based composites obtained in Examples 1 and 2 using nano-MgO particles. Therefore, the present invention significantly improves material performance over the existing patents.

[0079] Comparative Example 4: A method for preparing ultrafine-grained materials by low-temperature slow extrusion disclosed in a document 1

[0080] Pan et al. reported a method for producing ultrafine-grained Mg-Ca alloys at an extrusion rate of 0.5 mm / s in the range of 230-350°C (Mater Lett 2019; 237:65). The yield strength and elongation of the two low-alloyed magnesium alloys involved in this method were 377 MPa and 2% for the Mg-1.02Ca alloy and 290 MPa and 13% for the Mg-0.13Ca alloy, respectively. The materials reported in this paper failed to achieve both high mechanical properties and excellent elongation. Their mechanical properties and elongation were lower than those of Examples 1 and 2 of the present invention, which were 377 MPa and 10.1% and 435 MPa and 5.5%, respectively.

[0081] Comparative Example 5: A method for preparing ultrafine-grained materials by low-temperature slow extrusion disclosed in a document 2

[0082] Li et al. reported a method for preparing ultrafine-grained Mg-1Ca-1Al-0.3Zn-0.4Mn alloy at 300°C and an extrusion rate of 0.4 mm / s (Mater Charact 2021; 175: 111049). The yield strength and elongation of the Mg-1Ca-1Al-0.3Zn-0.4Mn alloy involved in this method were 435 MPa and 4.9%, respectively.

[0083] Compared with Example 2 of the present invention, although the material properties are similar, the magnesium alloy involved in the above method contains a significantly higher content of alloying elements other than magnesium. The higher content of alloying elements other than magnesium will often cause a large amount of intermetallic compounds to form in the alloy matrix. These intermetallic compounds will inhibit grain boundary migration during extrusion and promote the formation of ultrafine-grained structures. However, these intermetallic compounds will also accelerate the corrosion of the alloy, which is obviously not conducive to improving the corrosion resistance of the alloy. In comparison, the nano-MgO particle-controlled ultrafine-grained magnesium-based composite materials prepared in Examples 1 and 2 of the present invention not only have the high strength of the above-mentioned ultrafine-grained alloys, but also have high toughness (high elongation) and low alloying, effectively avoiding rapid corrosion caused by intermetallic compounds and improving corrosion resistance.

[0084] Comparative Example 6: A method for preparing ultrafine-grained materials by low-temperature slow extrusion disclosed in a document 3

[0085] Nie et al. reported a method for preparing ultrafine-grained Mg-4Zn-0.5Ca-0.5TiC composites at an extrusion rate of 2.4 mm / s in the range of 270-310 °C (T Nonferr Metal Soc 2020; 30: 2394). The yield strength and elongation of the Mg-4Zn-0.5Ca-0.5TiC composites involved in this method were 404 MPa and 5.2%, respectively.

[0086] Despite having a high content of alloying elements other than magnesium (including TiC particles), the composite materials reported above still failed to achieve both high mechanical properties and excellent elongation. Their mechanical properties and elongation were inferior to those of the ultrafine-grained magnesium-based composite materials obtained in Examples 1 and 2 of the present invention, which were controlled by nano-MgO particles.

[0087] The self-protected, degradable MgO / Mg-Zn-Ca biocomposite in Comparative Example 3 has a higher content of alloying elements other than magnesium than those in Examples 1-2, but its mechanical properties are still inferior to those of the nano-MgO particle-controlled ultrafine-grained magnesium-based composite material of the present invention. Furthermore, Comparative Examples 4-6 also demonstrate that, using existing reported methods, it is difficult to prepare low-alloyed magnesium-based composite materials with both high yield strength and high elongation through extrusion. This demonstrates that the present invention can produce nano-MgO particle-controlled ultrafine-grained magnesium-based composite materials with high strength, high elongation, and high corrosion resistance.

[0088] The present invention enhances the ability of dynamic recrystallization during hot extrusion and inhibits grain boundary migration during hot extrusion by adding nano-MgO particles. This allows for more complete dynamic recrystallization during the hot extrusion process (extrusion temperature of 150°C to 400°C, extrusion rate of 0.01mm / s to 1.0mm / s, and extrusion ratio of 10:1 to 60:1), resulting in a fully recrystallized ultrafine-grained structure. Furthermore, the synergistic effect of the grain boundary segregation of solute elements and the dynamic precipitation of high-density nano-second phase particles during the hot extrusion process effectively pins the grain boundaries, preserving the dynamically recrystallized ultrafine-grained structure at high temperatures. The nano-MgO particles control the proportion of recrystallized grains in the ultrafine-grained magnesium-based composite material to be greater than 75%, the average grain size to be less than 1μm, the mechanical properties to be greater than 376MPa, and the average annual corrosion rate to be no higher than 0.81mm / y after a 28-day standard immersion test using SBF solution according to ASTM G31-72.

[0089] By comprehensively optimizing material composition and improving the hot extrusion process, the present invention utilizes the principles of dynamic recrystallization and dynamic precipitation of nano-second phases during the hot extrusion process to create a simple process flow for the continuous, large-scale production of high-strength, high-toughness, high-corrosion-resistant, low-alloyed magnesium alloys with an ultrafine-grained structure. This method enables the controlled preparation of high-strength, high-toughness, and high-corrosion-resistant ultrafine-grained magnesium-based composite materials. The process is short, requiring only a single hot extrusion treatment of the magnesium-based composite material to obtain the ultrafine-grained structure. This method also enables the continuous production of rods, resulting in high production efficiency and suitability for large-scale industrial production. The processing method of the present invention produces uniformly sized, equiaxed ultrafine-grained structures with a high degree of grain recrystallization, excellent mechanical properties, and excellent corrosion resistance.

[0090] The above is an exemplary description of the present invention. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by other skilled in the art without expending creative labor falls within the scope of protection of the present invention.

Claims

1. A method for processing ultrafine-grained magnesium-based composite materials by nano-MgO particles, characterized in that: The nano-MgO particles regulate the grain size of ultrafine-grained magnesium-based composite materials d 100 nm< d <1 μm, the processing method includes the following steps: S1: obtaining a cast magnesium-based composite material, wherein the cast magnesium-based composite material consists of 1wt% Zn, 0.2wt% Ca, 1wt% MgO and the remainder Mg, in terms of mass percentage, wherein the MgO is nano-MgO particles, and the average diameter of the nano-MgO particles is less than 100 nm; S2: keeping the cast magnesium-based composite material at a first preset temperature for at least 4 hours, and cooling it in warm water to obtain a solid solution magnesium-based composite material, wherein the first preset temperature is 350-550°C, the holding time of the first preset temperature is 4-36 hours, and the temperature of the warm water is 60-70°C; S3: hot-extrude the solid solution magnesium-based composite material and cool it at room temperature to obtain an ultrafine-grained magnesium-based composite material regulated by nano-MgO particles, wherein the hot extrusion temperature is 260-270 °C and the hot extrusion rate is 0.01-0.1 mm / s.

2. The processing method according to claim 1, characterized in that: In S3, the extrusion ratio of the hot extrusion is (10~60):1.