A method for removing heat from EPVA polymerization under low pressure conditions and a method for preparing EPVA

By treating the gas phase and liquid phase concurrently in the polymerization reaction of EPVA, condensate and non-condensate gases and returning them to the reaction environment, the problem of low heat removal efficiency of gas phase ethylene under low pressure is solved, and high efficiency removal of low energy consumption is achieved Heat ensures the smooth progress of the reaction during EPVA synthesis.

CN115991810BActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111217469.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-19
Publication Date
2024-11-01
Estimated Expiration
2041-10-19

AI Technical Summary

Technical Problem

When synthesizing ethylene modified polyvinyl alcohol (EPVA) under low pressure conditions, the efficiency of using gas-phase ethylene for heat removal is not high and the energy consumption is large, so it cannot effectively remove the heat generated by the polymerization reaction.

Method used

By flowing the gas phase part and the liquid phase part in the polymerization reaction and cooling treatment is performed in the heat exchanger, condensate and non-condensate gas are formed, and the condensate is returned to the reaction environment, and the non-condensate gas treated by the pressurized process also returns to the Transport the reaction environment to achieve effective heat removal.

Benefits of technology

Under low polymerization pressure (such as 1 bar), the reaction heat is efficiently removed, energy consumption is reduced, and the use of harsh cooling conditions is not required, which can achieve efficient preparation of EPVA and improve the heat removal efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115991810B_ABST
    Figure CN115991810B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of ethylene-modified polyvinyl alcohol preparation methods, and specifically to a method for removing heat from EPVA polymerization under low-pressure conditions and a method for preparing EPVA and equipment thereof. A method for preparing EPVA under low-pressure conditions, wherein a copolymerization system is subjected to a polymerization reaction in a reaction environment to obtain a copolymer resin; during the polymerization reaction, a gas phase portion composed of ethylene, vinyl ester compounds and solvents is extracted from the reaction environment and flows in parallel with a liquid phase portion composed of vinyl ester compounds and solvents, and then a condensate and a non-condensable gas are formed after a temperature reduction treatment; the condensate is transported back to the reaction environment, and the non-condensable gas is transported back to the reaction environment after a pressurized treatment; and a polymerization liquid containing the copolymer resin is continuously collected from the reaction environment. This scheme can solve the technical problem of low efficiency in removing heat using gas-phase ethylene when synthesizing EPVA under low-pressure conditions, and can be applied to the practical operation of EPVA production and preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ethylene-modified polyvinyl alcohol preparation method, and in particular to a method for removing heat from EPVA polymerization under low pressure conditions and a method for preparing EPVA and equipment thereof. Background Art

[0002] Ethylene-modified polyvinyl alcohol (EPVA) is a modified polyvinyl alcohol obtained by preparing ethylene-vinyl acetate copolymer by copolymerization of vinyl acetate (VAC) and ethylene, and then alcoholysis. In order to ensure the water solubility of EPVA, EPVA with low ethylene content is preferred, which requires the use of a lower polymerization pressure, such as 1-15 bar, during the polymerization reaction to synthesize a polymer product with low ethylene content. The reaction of copolymerization of vinyl acetate (VAC) and ethylene is an exothermic reaction, and the heat generated during the reaction needs to be removed in time to ensure the smooth progress of the reaction. However, the temperature of the above-mentioned polymerization reaction is 30-90 ° C, and the raw material solvent and vinyl acetate of the polymerization reaction cannot be azeotropic, and it is impossible to remove heat by conventional heat removal methods. If gas phase ethylene is used for heat removal, at a polymerization pressure of 1-15 bar, the phase transition temperature of ethylene is very low, resulting in low condensation heat removal efficiency and high heat removal energy consumption. How to use gas phase ethylene to effectively remove heat during the synthesis of EPVA with low ethylene content is a problem to be solved urgently, and it is urgent to develop a method and equipment that can improve heat removal efficiency and reduce energy consumption. Summary of the invention

[0003] The present invention is intended to provide a method for preparing EPVA under low pressure conditions to solve the technical problem of low efficiency of heat removal using gas phase ethylene when synthesizing EPVA under low pressure conditions.

[0004] In order to achieve the above object, the present invention adopts the following technical scheme:

[0005] A method for preparing EPVA under low pressure conditions, comprising a polymerization reaction step: a copolymerization system is subjected to a polymerization reaction in a reaction environment to obtain a copolymer resin; the raw materials of the copolymerization system include ethylene, a vinyl ester compound, a solvent and an initiator; the copolymerization system includes a polymerization liquid and a gas phase part composed of ethylene, a vaporized vinyl ester compound and a vaporized solvent;

[0006] During the polymerization reaction, the gas phase is discharged from the reaction environment and flows concurrently with the liquid phase composed of vinyl ester compounds and solvents, and then forms condensate and non-condensable gas after cooling treatment; the condensate is transported back to the reaction environment, and the non-condensable gas is transported back to the reaction environment after pressurization treatment; and the polymerization liquid containing the copolymer resin is continuously collected from the reaction environment.

[0007] The present scheme also provides an apparatus for preparing EPVA under low-pressure conditions, comprising a polymerization kettle and a heat exchanger; the upper portion of the polymerization kettle is connected to a gas phase conduit, the other end of the gas phase conduit is connected to the inlet of the material channel of the heat exchanger, and the inlet of the material channel of the heat exchanger is also connected to a liquid phase conduit for introducing a solvent and a second monomer; the material channel of the heat exchanger comprises a non-condensable gas outlet and a condensate outlet, the condensate outlet is connected to the upper portion of the polymerization kettle through the condensate conduit, the non-condensable gas outlet is connected to the upper portion of the polymerization kettle through the non-condensable gas conduit, and a circulating press is provided on the non-condensable gas conduit; the upper portion of the polymerization kettle is also connected to a feed pipe, and the bottom of the polymerization kettle is also provided with a polymerization liquid discharge port.

[0008] The present scheme also provides a method for removing heat from EPVA polymerization under low-pressure conditions, wherein ethylene, vinyl ester compounds, an initiator and a solvent are introduced into a reaction environment to form a copolymerization system; the copolymerization system includes a gas phase portion consisting of ethylene, vinyl ester compounds and a solvent; the gas phase portion is mixed in parallel with a liquid phase portion consisting of vinyl ester compounds and a solvent to form a mixed fluid; the mixed fluid is cooled to form a condensate and a non-condensable gas, the condensate is directly drained back to the reaction environment, and the pressurized non-condensable gas is drained back to the reaction environment.

[0009] The principle and advantages of this scheme are: this scheme prepares ethylene-vinyl acetate copolymer by solution polymerization of ethylene and vinyl acetate, and provides a preparation method suitable for low-content ethylene-modified polyvinyl alcohol, and can efficiently remove the reaction heat in the EPVA polymerization process even when the polymerization pressure is as low as 1 bar. The present invention can efficiently remove the reaction heat in the EPVA polymerization process even when the polymerization pressure is as low as 1 bar, perfectly solving this technical problem, which is of great significance.

[0010] The method for achieving effective heat removal in this scheme is specifically as follows: ethylene, vinyl ester compounds, solvents and initiators form a copolymerization system. The copolymerization system in the polymerization kettle is divided into a polymerization liquid and a gas phase composed of ethylene, vaporized vinyl ester compounds and vaporized solvents due to the nature of the materials. This scheme draws the gas phase out of the reaction environment and makes it flow in parallel with the liquid phase composed of vinyl ester compounds and solvents, which plays a role in further dissolving the ethylene in the gas phase and cooling the temperature. After the parallel flow, after the cooling treatment of the heat exchanger, a condensate with a lowered temperature and a non-condensable gas are formed, and the condensate is transported back to the reaction environment, and the non-condensable gas is transported back to the reaction environment after pressurization treatment. The above method can achieve effective heat removal of the reaction system without using harsh cooling conditions (only 0-33°C cooling water is used at the heat exchanger, and no low-temperature cooling medium is used). During the polymerization process, if gaseous ethylene is used for heat removal, the phase transition temperature of ethylene is very low at a polymerization pressure of 1-15 bar, and a very low temperature cooling medium is required to treat the ethylene, resulting in low condensation heat removal efficiency and high heat removal energy consumption. The use of this technical solution overcomes the problems existing in the prior art and can achieve effective heat removal of the reaction system with low energy consumption.

[0011] Furthermore, the flow ratio of the gas phase part and the liquid phase part is 5-15:0.5-3; the temperatures of the condensate and the non-condensable gas formed after the cooling treatment are 30-50°C and 30-90°C respectively; the temperature of the liquid phase part is 0-30°C. The flow rates of the gas phase part and the liquid phase part are controlled within the above range, and the temperature of the liquid phase part is 0-30°C. When the mixture composed of the gas phase part and the liquid phase part is cooled by 0-33°C cooling water, the temperatures of the condensate and the non-condensable gas formed can be reduced to 30-50°C and 30-90°C respectively. The two parts are introduced back into the reaction environment, so that the recycling of materials can be realized, and the purpose of effectively withdrawing the heat generated by the reaction can be achieved.

[0012] Furthermore, the pressure of the reaction environment is 1-15 bar and the temperature is 30-150°C.

[0013] Furthermore, the pressure of the reaction environment is 1-10 bar and the temperature is 30-90°C.

[0014] At a reaction pressure of 1-15 bar and a temperature of 30-150°C, ethylene-vinyl acetate copolymers with low ethylene content can be synthesized, and then alcoholysis is performed to obtain ethylene-modified polyvinyl alcohol with good solubility. At a reaction pressure of 1-10 bar and a temperature of 30-90°C, the solubility of the synthesized ethylene-modified polyvinyl alcohol is even better, meeting the application requirements.

[0015] Furthermore, the mass ratio of the vinyl ester compound, the initiator and the solvent is 20-80: 0.0001-0.1: 2-50. The above material ratio can ensure the smooth progress of the reaction.

[0016] Furthermore, the vinyl ester compound includes at least one of vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, trimethylacetate, vinyl octanoate, vinyl laurate, vinyl stearate and benzyl vinyl ester; the initiator is one of an azo initiator, a peroxide initiator and a redox initiator; the solvent is methanol, ethanol or isopropanol. Using the above raw materials, an ethylene-vinyl acetate copolymer that meets the requirements can be synthesized according to specific needs.

[0017] Furthermore, the raw materials of the copolymerization system also include a solvent and a third monomer; the third monomer includes at least one of vinyl unsaturated sulfonic acid and its alkyl ester, vinyl unsaturated carboxylic acid compounds and alkyl vinyl ether. The third monomer can be added to the ethylene-vinyl acetate copolymer according to product requirements.

[0018] Furthermore, the copolymer resin is subjected to alcoholysis reaction under the action of a catalyst to obtain ethylene-modified polyvinyl alcohol; the catalyst is one of sodium hydroxide, potassium hydroxide, sulfuric acid, hydrochloric acid and p-toluenesulfonic acid. The ethylene-vinyl acetate copolymer is subjected to alcoholysis treatment to obtain an ethylene-modified polyvinyl alcohol final product. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of the EPVA polymerization equipment of Example 1 of the present invention. DETAILED DESCRIPTION

[0020] The following is further described in detail through specific implementation methods:

[0021] The figure marks in the drawings of the specification include: a first feed pipe 1, a second feed pipe 2, a third feed pipe 3, a fourth feed pipe 4, a polymerization kettle 5, a heat exchanger 6, a liquid phase conduit 7, a gas phase conduit 8, a non-condensable gas conduit 9, a water supply conduit 10, a return water conduit 11, a circulating press 12, a polymerization liquid discharge port 13, and a condensate conduit 14.

[0022] Embodiment 1:

[0023] like Figure 1As shown, the EPVA polymerization equipment includes a polymerization kettle 5 and a heat exchanger 6. The upper part of the polymerization kettle 5 is connected with a first feed pipe 1, a second feed pipe 2, a third feed pipe 3 and a fourth feed pipe 4. The first feed pipe 1, the second feed pipe 2, the third feed pipe 3 and the fourth feed pipe 4 are respectively used for feeding the solvent, the first monomer (ethylene), the second monomer (vinyl ester compound) and the initiator. A polymerization liquid discharge port 13 is provided at the bottom of the polymerization kettle 5. The heat exchanger 6 is a conventional heat exchanger, in which a material channel and a cooling medium channel are provided. The material and the cooling medium are separated by a solid partition wall, and heat exchange is performed through the partition wall. The inlet of the cooling medium channel is connected with a water supply conduit 10, and the outlet is connected with a return water conduit 11. Cooling water flows in the cooling medium channel. The inlet of the material channel is located at the upper part of the heat exchanger 6, including a liquid phase inlet and a gas phase inlet; the outlet of the material channel is located at the lower part of the heat exchanger 6, including a non-condensable gas outlet and a condensate outlet. The upper part of the polymerization kettle 5 is also connected with a gas phase conduit 8, a non-condensable gas conduit 9 and a condensate conduit 14. The end of the gas phase conduit 8 away from the polymerization kettle 5 is connected to the gas phase inlet of the material channel, and the liquid phase inlet of the material channel is connected to the liquid phase conduit 7. The materials in the liquid phase conduit 7 and the gas phase conduit 8 are mixed in the material channel. The end of the condensate conduit 14 away from the polymerization kettle 5 is connected to the condensate outlet of the material channel. The end of the non-condensable gas conduit 9 away from the polymerization kettle 5 is connected to the non-condensable gas outlet of the material channel, and a circulating compressor 12 is arranged on the non-condensable gas conduit 9. During the polymerization reaction, the gas phase part composed of the first monomer, the second monomer (gasified) and the solvent (gasified) continuously enters the heat exchanger 6 from the gas phase conduit 8, and the liquid phase part composed of the second monomer and the solvent continuously enters the heat exchanger 6 from the liquid phase conduit 7. The liquid phase part composed of the second monomer and the solvent is in parallel contact with the gas phase part composed of the first monomer, the second monomer and the solvent in the heat exchanger 6, and the liquid phase part composed of the second monomer and the solvent absorbs the first monomer, the second monomer and the solvent in the gas phase part. Cooling water is continuously introduced into the heat exchanger 6, so that the solvent and the second monomer in the gas phase composed of the first monomer, the second monomer and the solvent continuously flow to the polymerization kettle 5 through the condensate conduit 14. The first monomer in the gas phase composed of the first monomer, the second monomer and the solvent that has not been condensed and absorbed is continuously introduced back to the polymerization kettle 5 through the non-condensable gas conduit 9 and the circulation compressor 12. The polymer liquid is continuously discharged from the polymerization kettle 5 discharge port 13 to keep the liquid level unchanged.

[0024] When preparing ethylene-modified polyvinyl alcohol, a first monomer and a second monomer, an initiator and a solvent are added to a polymerization kettle 5. The first monomer is ethylene. The second monomer includes at least one of vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, trimethylacetic acid vinyl ester, vinyl octanoate, vinyl laurate, vinyl stearate and benzyl vinyl ester. The solvent is an alcohol solvent, including methanol, ethanol or isopropanol. The initiator is one of an azo initiator, a peroxide initiator and a redox initiator. Azo initiators are azobisisobutyl cyanide (ABIN) or azobisisoheptyl cyanide (ABVN); peroxide initiators are bis(4-tert-butylcyclohexyl) peroxydicarbonate (Perkadox16), tert-pentyl peroxypivalate (PV-75), bis(2-ethylhexyl) peroxydicarbonate (EHP), bis(3,5,5-trimethylhexanoyl) peroxide (Trigonox 36) or dipropyl peroxydicarbonate (NPP-50); redox initiators are potassium persulfate, ammonium persulfate, sodium bisulfite, sodium bicarbonate, tartaric acid or Rongalite. Potassium persulfate and ammonium persulfate are peroxide oxidants, and sodium bisulfite, sodium bicarbonate, tartaric acid and Rongalite are reducing agents.

[0025] The reaction substrate may also include a third monomer, the third monomer including at least one of ethylene unsaturated carboxylic acid compounds, alkyl vinyl ethers, ethylene unsaturated sulfonic acids and alkyl esters thereof. The ethylene unsaturated carboxylic acid compounds include at least one of methacrylic acid, butenoic acid, anhydrous maleic acid, fumaric acid, itaconic acid and alkali metal salts thereof. The alkyl vinyl ether includes at least one of propyl vinyl ether, octyl vinyl ether, decyl vinyl ether and dodecyl vinyl ether. The ethylene unsaturated sulfonic acid and alkyl ester thereof include at least one of methyl butenoate, ethyl butenoate, methyl itaconate, ethyl itaconate, methyl sorbate, ethyl sorbate, monoalkyl maleate, dialkyl maleate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate and heptyl methacrylate.

[0026] The pressure of the polymerization reaction of the materials in the polymerization reactor 5 is 1-15 bar (polymerization pressure). The lower the polymerization pressure, the lower the ethylene content of the prepared EPVA. In order to ensure the water solubility of EPVA, EPVA with low ethylene content is preferred, and the polymerization pressure is preferably below 10 bar (for example, 1.5-10 bar). The polymerization temperature (polymerization temperature) is 30-150° C., preferably 30-90° C. The pressure is maintained within a specified range in the polymerization reactor 5 by introducing a certain amount of ethylene.

[0027] More specifically, the case where the second monomer is vinyl acetate and the solvent is methanol is further described, and the first monomer used specifically is ethylene. During the polymerization reaction, heat is removed through the heat exchanger 6, and the gas phase part (composed of ethylene, vaporized vinyl acetate and vaporized methanol) in the polymerization system is continuously introduced into the heat exchanger 6 from the gas phase conduit 8. At the same time, the liquid phase part composed of vinyl acetate and methanol (temperature is 0-30°C, the mass ratio of vinyl acetate and methanol is 20-80:2-30, and 2:3 is specifically used in the following embodiments) continuously enters the heat exchanger 6 from the liquid phase conduit 7. The flow ratio of the gas phase part and the liquid phase part is 5-15:0.5-3. The gas phase part and the liquid phase part are in parallel contact in the heat exchanger 6, and heat exchange is carried out in the heat exchanger 6. The cooling medium used in the heat exchanger 6 is water, the water temperature of the water in the water supply conduit 10 is 0-33°C, and the water temperature of the water in the return water conduit 11 is 10-43°C. After heat exchange, condensate (mainly containing vinyl acetate and methanol, as well as dissolved ethylene, with a temperature of 30-50°C) and non-condensable gas (mainly ethylene, with a temperature of 30-90°C) are formed, and the condensate flows continuously to the polymerization kettle 5 through the condensate conduit 14, and the non-condensable gas is continuously guided back to the polymerization kettle 5 through the non-condensable gas conduit 9 and the circulation compressor 12. The circulation compressor 12 increases the pressure of the non-condensable gas to 1-15 bar (preferably 1.5-10 bar), so that the pressure of the non-condensable gas is increased to the same as the pressure in the polymerization kettle 5, and then returns to the polymerization kettle 5, and the polymerization liquid in the polymerization kettle 5 continuously flows out from the polymerization liquid discharge port 13, and the copolymerization product (containing the copolymer resin) is collected from the polymerization liquid discharge port 13, and the liquid level in the polymerization kettle 5 is kept unchanged. The polymerization kettle 5 is a conventional continuous reactor, in which the residence time of the reaction materials is 8-12 hours. The liquid level of the polymerization kettle 5 remains unchanged during the reaction, which is achieved by regulating the speed at which the polymerization liquid continuously flows out from the polymerization liquid outlet 13, and the feeding speed of the first feed pipe 1, the second feed pipe 2, the third feed pipe 3 and the fourth feed pipe 4. The first feed pipe 1, the second feed pipe 2, the third feed pipe 3 and the fourth feed pipe 4 are used for feeding the solvent, the first monomer (ethylene), the second monomer (vinyl ester compound) and the initiator respectively. In the polymerization reaction, the feeding amount ratio (mass ratio) of the vinyl ester compound, the initiator and the solvent is 20-80: 0.0001-0.1: 2-50. The pressure in the polymerization kettle 5 is maintained within a specified range, i.e., 1-15 bar (preferably 1.5-10 bar) by introducing a certain amount of ethylene.

[0028] The polymer solution is blown out of the residue to obtain a methanol solution of polyvinyl acetate, the mass fraction of polyvinyl acetate is adjusted to 10-30%, a catalyst is added for alcoholysis, and the polyvinyl alcohol powder is obtained by drying and crushing. The alcoholysis method can be any process method such as intermittent, semi-continuous, and continuous. The temperature of the alcoholysis reaction is 10-70°C, preferably 30-50°C. The catalyst is sodium hydroxide, potassium hydroxide, sulfuric acid, hydrochloric acid or p-toluenesulfonic acid, sodium hydroxide and potassium hydroxide are alkaline catalysts; sulfuric acid, hydrochloric acid and p-toluenesulfonic acid are acidic catalysts. The amount of the catalyst is 0.0007-0.1 molar equivalent of the copolymer resin. The solvent for the alcoholysis reaction is a solvent with a dielectric constant of less than 30, preferably methanol.

[0029] Example 2

[0030] The synthesis of ethylene-vinyl acetate copolymer under polymerization pressure conditions of 1.5 bar, 5 bar, 10 bar, and 15 bar is used as an example for explanation. The synthesis process is shown in Example 1, and the specific parameter selection is shown in Table 1. The criterion for judging whether the heat removal is effective is: the polymerization reaction is carried out continuously for 10 hours or longer, and the temperature change in the polymerization kettle 5 during the period does not exceed 5°C; if the temperature change in the polymerization kettle 5 exceeds 5°C, and the polymerization reaction has not been carried out for 10 hours, the reaction needs to be stopped in advance. The feed ratio in Table 1 refers to the feed ratio of ethylene, vinyl ester compound (vinyl acetate), initiator and solvent (methanol). After the non-condensable gas is pressurized, its pressure is consistent with the pressure in the reactor, and then it returns to the polymerization kettle 5.

[0031] Table 1: Experimental parameter selection and experimental results

[0032]

[0033] Experiments No. 1-4 can achieve effective heat removal during the polymerization reaction, and only 0-33°C circulating water is needed in the heat exchanger 6, without the need for a low-temperature cooling medium, which saves more energy. In Experiment No. 5, the amount of liquid phase used is too small and the temperature is relatively high, so effective heat removal cannot be achieved during the reaction. When the reaction is carried out for 4 hours, the temperature rise in the polymerization kettle 5 has exceeded 5°C. A cooling medium with a lower temperature needs to be used in the heat exchanger 6 to achieve effective heat removal, which is a waste of energy. In Experiment No. 6, the non-condensable gas is no longer introduced back into the polymerization kettle 5 after the heat exchange, making it difficult to achieve effective heat removal. When the reaction is carried out for 3 hours, the temperature rise in the polymerization kettle 5 has exceeded 5°C.

[0034] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing EPVA under low pressure conditions, characterized in that: The method comprises the steps of polymerization reaction: a copolymerization system is subjected to polymerization reaction in a reaction environment to obtain a copolymer resin; the raw materials of the copolymerization system include ethylene, a vinyl ester compound, a solvent and an initiator; the copolymerization system includes a polymerization liquid and a gas phase part composed of ethylene, a vaporized vinyl ester compound and a vaporized solvent, and the mass ratio of the vinyl ester compound, the initiator and the solvent is 20-80: 0.0001-0.1:2-50; During the polymerization reaction, the gas phase is led out from the reaction environment and flows in parallel with the liquid phase composed of vinyl ester compounds and solvents, and then forms condensate and non-condensable gas after cooling treatment; the condensate is transported back to the reaction environment, and the non-condensable gas is transported back to the reaction environment after pressurization treatment; and the polymerization liquid containing the copolymer resin is continuously collected from the reaction environment; the flow ratio of the gas phase and the liquid phase is 5:0.5-3; The temperatures of the condensate and non-condensable gas formed after the cooling treatment are 30-50°C and 30-90°C respectively; the temperature of the liquid phase is 0-30°C; the pressure of the reaction environment is 1-15 bar and the temperature is 30-150°C.

2. The method for preparing EPVA under low pressure according to claim 1, characterized in that: The pressure of the reaction environment is 1-10 bar and the temperature is 30-90°C.

3. The method for preparing EPVA under low pressure according to claim 2, characterized in that: The vinyl ester compound includes at least one of vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, trimethylacetate, vinyl octanoate, vinyl laurate, vinyl stearate and benzyl vinyl ester; the initiator is one of an azo initiator, a peroxide initiator and a redox initiator; and the solvent is methanol, ethanol or isopropanol.

4. The method for preparing EPVA under low pressure conditions according to claim 3, characterized in that: The raw materials of the copolymerization system further include a solvent and a third monomer; the third monomer includes at least one of vinyl unsaturated sulfonic acid and its alkyl ester, vinyl unsaturated carboxylic acid compounds and alkyl vinyl ether.

5. The method for preparing EPVA under low pressure conditions according to claim 4, characterized in that: The copolymer resin undergoes alcoholysis reaction under the action of a catalyst to obtain ethylene-modified polyvinyl alcohol; the catalyst is one of sodium hydroxide, potassium hydroxide, sulfuric acid, hydrochloric acid and p-toluenesulfonic acid.