Composite material leaf spring and preparation method thereof

By winding a large area of ​​prepreg to form a multi-layer circumferential fiber structure, the problem of layered failure of composite leaf springs under complex loads in the prior art is solved, and efficient and low-cost production is achieved. Meet the application needs of the automotive industry.

CN116001307BActive Publication Date: 2024-11-08NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111231568.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-22
Publication Date
2024-11-08
Estimated Expiration
2041-10-22

AI Technical Summary

Technical Problem

Existing composite leaf springs are prone to stratified damage under complex loads such as large torsion loads, humidity and heat, high and low temperatures and fatigue, making them difficult to serve for a long time, and have high production efficiency and cost.

Method used

A large area of ​​prepreg is wound into a prefabricated tube, and is pressurized and cured by repeated composite mold pressurization and mold pressurization to form a composite leaf spring with multi-layer circumferential fiber structure to avoid layered cracking, and the core surface is cleaned by alcohol. , use a soft material pipe roller and a vacuum pump to improve density and efficiency.

Benefits of technology

It realizes the high fatigue resistance and long service life of composite leaf springs under complex working conditions, while greatly improving production efficiency, reducing manufacturing costs, and meeting the low-cost, large-scale mass production needs of the automotive industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116001307B_ABST
    Figure CN116001307B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a composite leaf spring, comprising: winding and compressing a prepreg composite material on the surface of a core material, and then extracting the core material to obtain a prefabricated tube; placing the prefabricated tube into a preforming mold, and at room temperature, pressurizing the mold, wherein the pressurizing pressure is 2-5MPa, to obtain a prefabricated part; placing the prefabricated part into a forming mold, pressurizing, and demolding to obtain a composite leaf spring. The method is efficient, low in cost, and suitable for large-scale mass production. The present invention also provides a composite leaf spring prepared by the method, wherein the composite leaf spring has high fatigue resistance and can withstand high bending loads and torsional loads at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leaf spring manufacturing, and in particular to a method for preparing a composite leaf spring. Background Art

[0002] Lightweighting of automobiles is an important measure for my country to achieve energy conservation, emission reduction and environmental protection. Fiber-reinforced resin-based composite materials have the advantages of light weight, high strength, fatigue resistance, corrosion resistance and strong designability, and are ideal materials for achieving lightweighting of automobiles.

[0003] Resin-based composite materials have the advantages of high specific strength, high specific modulus, strong design, good high-temperature performance, simple manufacturing process and low cost. Practice has proved that the use of composite materials in automobiles can effectively reduce the weight of the car and reduce fuel consumption, thereby reducing the cost of use and reducing pollution to the environment, which is of great significance to achieving sustainable development. The use of composite materials instead of steel plates to manufacture commercial vehicles and freight truck leaf springs has been verified by automobile companies and has achieved good lightweight effects such as vibration reduction and fuel saving. The current molding processes of composite leaf springs mainly include prepreg molding, winding, high-pressure RTM, pultrusion and three-dimensional weaving.

[0004] The Chinese patent with the patent number CN109228398B discloses a method for cutting a whole block of leaf spring prepreg after stacking layer by layer, comprising the following production steps: a: blank making, stacking prepreg on a stacking mold, and then cutting the prepreg to form a whole block of blanks; b: whole block blank cutting, cutting the whole block blank along the length direction of the leaf spring, cutting the whole block blank into several single blanks, the width of the single blank is the width of the leaf spring; c: mold entry, placing the cut single blank into a preforming mold for pre-compaction to form a preformed leaf spring; d: oven preheating, placing the preformed leaf springs in an oven in turn and heating them to a predetermined temperature required by the process; e: molding and curing, placing the preformed leaf spring heated to a predetermined temperature into a press for heating and pressurization curing; f: demolding, removing the cured leaf spring from the mold. This method can improve the production efficiency of leaf springs, but the prepared leaf springs are all simple laminated structures. There are no continuous annular wrapped fibers in the thickness direction, which can easily cause delamination damage under large torsional loads and cannot adapt to the complex use scenarios of cars on bumpy roads for a long time.

[0005] A Chinese patent with patent number CN110667135A discloses a method for preparing a leaf spring preform by a "folding and wrapping method", comprising: the folding and wrapping method forms a preform by continuously folding a prepreg in the width direction and wrapping it in the circumferential direction. This method effectively improves the torsional resistance of the composite leaf spring and greatly improves the production efficiency. However, there are problems with the compatibility and long-term bonding reliability between the nylon core strip and the epoxy resin used. Delamination failure is prone to occur under the coupling of multiple complex loads such as moisture, heat, high and low temperatures, and fatigue, which poses a hidden danger to the long-term service performance of the composite leaf spring.

[0006] Therefore, there is an urgent need to design a high-efficiency and low-cost preparation method for composite leaf springs that can avoid delamination damage and can serve for a long time under the coupling of multiple complex loads such as large torsional loads, moisture and heat, high and low temperatures, and fatigue. Summary of the invention

[0007] The present invention provides a method for preparing a composite leaf spring. The method is efficient, low in cost, and suitable for large-scale mass production. The composite leaf spring prepared by the preparation method has high fatigue resistance and can withstand high bending loads and torsional loads at the same time.

[0008] A method for preparing a composite leaf spring, comprising:

[0009] (1) Winding and pressing the prepreg on the surface of the core material, and then extracting the core material to obtain a prefabricated tube;

[0010] (2) placing the prefabricated tube into a preforming mold, and applying pressure to the preforming mold at room temperature, wherein the pressure is 2-5 MPa, to obtain a prefabricated part;

[0011] (3) placing the preform into a molding die, applying pressure, and demoulding to obtain a composite leaf spring.

[0012] The present invention uses a large area of ​​prepreg, which saves laying time and does not limit the cutting shape. Compared with the prior art that needs to cut into small-sized, slender prepregs, the number of cuts can be reduced from hundreds of pieces to dozens of pieces, thereby greatly saving cutting time; the present invention uses the method of winding the prepreg into a prefabricated tube, which has better integrity than the layer-by-layer stacking process disclosed in the prior art, is not easy to delaminate and crack under complex working conditions such as torsion and bending, and has higher load-bearing performance and service life than traditional products.

[0013] Before winding the prepreg on the surface of the core material, use alcohol and deionized water to clean the surface of the core material to make the surface clean, prevent impurities from damaging the load-bearing performance of the composite leaf spring in a harsh use environment, and do not spray release agent.

[0014] The prepreg is a unidirectional woven glass fiber prepreg, with a resin mass content of 30%-40% and a single layer thickness of 0.15mm-0.3mm.

[0015] The fiber layer angle of the prepreg is 0°-135°. Furthermore, the fiber angle of the prepreg composite material is 0°, 90°, 45° or 135°. The fiber layer angle is the angle between the fiber length direction of the prepreg after winding and the length direction of the composite leaf spring.

[0016] The prepreg wound on the surface of the core material comprises:

[0017] First, prepreg with a fiber angle of 0° is wound on the surface of the core material. When the winding thickness reaches more than 10 mm, continue to wind prepreg with a fiber angle of any angle between 0° and 135°.

[0018] The fiber winding angle on the surface of the core material provided by the present invention is 0°, which can eliminate the defects caused by the fibers being forced to bend in a small radius. Taking a fiber angle of 90 degrees as an example, when the winding is completed and the core material is removed, it will be forced to fold to 180 degrees during the next compaction process. The fiber is very rigid and is prone to breakage or residual voids at the small radius bends. These defects have a great negative impact on the fatigue performance of leaf springs. Using 0 degrees can avoid this. When the layer thickness reaches more than 10 mm, the bending radius of the fiber becomes larger, and small radius bending defects will not occur, so the first winding must be at an angle of 0°.

[0019] The area of ​​the prepreg is 0.3m*1m to 1.5m*3m.

[0020] The shape of the prepreg is square, rectangular, trapezoidal or triangular.

[0021] The shape of the prepreg is determined according to the thickness variation of the leaf spring. The constant thickness leaf spring is cut into square or rectangular prepreg, and the variable thickness leaf spring is cut into trapezoidal or triangular prepreg.

[0022] A tube reel with a soft surface is used to wind and compress the prepreg layer by layer on the surface of the core material. The heating temperature of the surface is 25℃-40℃ and the pressing force is 1MPa-3MPa. This is to eliminate the residual air between the layers and ensure that each winding layer is tightly fitted.

[0023] Furthermore, a 5-10 mm thick soft plastic such as polyurethane or silicone rubber is applied to the table surface to ensure that the prepreg in each layer and each part can be fully compressed when manufacturing the variable thickness composite leaf spring.

[0024] The core material is a cylindrical air bag, one end of which is connected to an air inlet valve and the other end is connected to an air outlet valve, and the core material is filled with gas. Furthermore, the air pressure in the core material is 1MPa-3MPa.

[0025] The process of extracting the core material to obtain a prefabricated tube comprises:

[0026] Open the exhaust valve to exhaust the gas in the core material, and then extract the core material to obtain a prefabricated tube. Further, the gas in the core material is extracted by a vacuum pump, and then the core material is extracted to obtain a prefabricated tube. This ensures that the wound prepreg does not deform or damage during the core removal process.

[0027] The core material is polyurethane or silicone rubber soft plastic.

[0028] The core material has a diameter of 10 mm to 30 mm and a length 100 mm to 200 mm longer than the composite material leaf spring.

[0029] The parameters of the reverse compound mold pressurization are: the preforming mold is a metal counter mold, the heating temperature is 30° C.-50° C., the pressure is 3-5 MPa, and the reverse compound mold is performed 2-3 times.

[0030] The preform is placed in a forming mold, pressurized, and demoulded to obtain a composite leaf spring, including:

[0031] The preform is placed in a molding mold for molding operation, and the resin of the prepreg is cured at a temperature of 100-150°C and a pressure of 10-20MPa to obtain a composite leaf spring blank. After demoulding, the flash is processed with a tool to finally obtain a composite leaf spring.

[0032] Rolling begins at one end or the middle of the preformed tube, and the gap between the rollers is gradually reduced to eliminate residual pores inside the preform.

[0033] The composite material leaf spring prepared by the method for preparing the composite material leaf spring is a leaf spring with constant thickness and constant cross-section, or a leaf spring with variable thickness and variable cross-section.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention cuts a large area of ​​prepreg at one time, instead of cutting slender prepreg in the traditional method, and the number of cuts can be reduced from hundreds of pieces to dozens of pieces, thus greatly saving cutting time.

[0036] The present invention adopts a tube winding machine to wind large-area prepreg into prefabricated tubes, instead of laying slender prepreg layer by layer in the traditional method, which can save more than 90% of the laying time and greatly improve the efficiency. The average molding time of a single product can be reduced from several hours to 10 to 15 minutes, meeting the large-scale and low-cost manufacturing requirements of the automotive industry.

[0037] The composite leaf spring manufactured by the method provided by the present invention has multiple layers and circumferential fibers, is not easy to delaminate and crack under complex working conditions such as torsion and bending, has higher load-bearing performance and service life than traditional products, has a torsional moment resistance of 50-80N·m, a fatigue life of 2.5-3 million times, and a bending load resistance of 60-90kN. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Schematic diagram of the efficient forming process of composite leaf springs of equal thickness or equal cross-section provided in Example 1.

[0039] Figure 2 Schematic diagram of the efficient forming process of a composite leaf spring with variable thickness or cross-section provided in Example 2.

[0040] Figure 3 This is a three-dimensional image of the composite leaf spring prepared in Example 2. DETAILED DESCRIPTION

[0041] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings so that the purpose, features and advantages of the present invention can be more clearly understood. It should be understood that the embodiments shown in the accompanying drawings are not intended to limit the scope of the present invention, but are only intended to illustrate the essential spirit of the technical solution of the present invention.

[0042] Example 1

[0043] A method for manufacturing composite leaf springs of uniform thickness or uniform cross-sectional shape, such as Figure 1 As shown:

[0044] First, cut the prepreg. Use an automatic cloth cutting machine to cut the unidirectional glass fiber prepreg into rectangular sheets, with a total of 50 sheets, including 35 sheets with the length direction of the sheet being the 0° direction of the fiber, with a size of 1200mm*1000mm; and 15 sheets with the length direction of the sheet being the 90° direction of the fiber, with a size of 1200mm*300mm. The cutting time takes 10-15 minutes.

[0045] Then make the prefabricated tube. Inflate the winding core mold airbag with an air pressure of 1MPa, and clean the surface with alcohol; use an automatic tube winding machine to wind the above cut prepreg sheets piece by piece, and the winding order is [0] 20 / [90 / 0] 15 That is, first wind 20 sheets of 0° sheets, and then alternately wind 15 sheets of 90° and 0° sheets. The temperature of the tube coiling machine table is 27°C, and the pressing force is 1.5MPa. After all the winding is completed, open the deflation valve at one end of the core mold to deflate the airbag and pull it out. If it is difficult to pull out, use a vacuum pump to evacuate the airbag. After the airbag shrinks, it can be smoothly pulled out to obtain a prefabricated tube.

[0046] Then put the prefabricated tube into the preforming mold, the mold temperature is 30℃, the mold is closed and slowly pressurized to 3MPa, and maintained for 10 minutes. During this period, the mold can be opened 2-3 times and pressurized again, which is conducive to removing the air remaining inside the material and improving the density of the composite leaf spring. After this operation, a leaf spring prefabricated part is obtained.

[0047] Finally, the preform is placed in the molding mold, the mold temperature is 120℃, the mold is closed and pressurized to 10MPa, and maintained for 30 minutes, and the resin completes the curing process. After demoulding, it is placed in an oven and post-cured at 150-180℃ for 2 hours to obtain a leaf spring blank. Use sandpaper to grind and remove the flash, and use a cutting tool to cut off the excess parts at both ends of the leaf spring if necessary. Finally, the finished composite leaf spring is obtained, such as Figure 2 shown.

[0048] The composite leaf springs of equal thickness and cross-section manufactured by the above method have an experimental bending failure load of 72kN, a torsional moment of 67N·m, and a fatigue life of 2.8 million times. The laying time of a single prepreg is only 30min, which is 90% less than the traditional prepreg manual layer-by-layer laying method, greatly improving production efficiency and reducing manufacturing costs, meeting the requirements of large-scale mass production applications in the automotive industry.

[0049] Example 2

[0050] The manufacturing method of the composite leaf spring with variable thickness or variable cross-sectional shape is as follows:

[0051] First, cut the prepreg. Use an automatic cloth cutting machine to cut the unidirectional glass fiber prepreg into rectangular and trapezoidal sheets, with a total of 50 sheets, including 15 rectangular sheets with a size of 1200mm*1000mm and a length direction of the fiber 0° direction; 15 rectangular sheets with a size of 1200mm*300mm and a length direction of the fiber 90° direction; 20 trapezoidal sheets with a size of 400mm upper bottom length, 1200mm lower bottom length, 1000mm trapezoid height, and the fiber 0° direction is parallel to the upper and lower bottom edges of the trapezoid. Cutting time takes 13-17 minutes.

[0052] Then make the prefabricated tube. Inflate the cylindrical airbag with an air pressure of 1MPa, and clean the surface with alcohol. Use an automatic tube reel to roll the above cut prepreg sheets piece by piece. First, roll 10 0° rectangular sheets; then alternately roll 20 trapezoidal sheets and 10 90° rectangular sheets, that is, after winding 2 layers of trapezoidal sheets, roll 1 layer of 90° rectangular sheets; finally, alternately roll the remaining 5 0° rectangular sheets and 5 90° rectangular sheets. The table temperature of the tube reel is 27°C, and the clamping force is 1.5MPa. After all the winding is completed, open the deflation valve at one end of the core mold to deflate the airbag and pull it out. If it is difficult to pull out, use a vacuum pump to evacuate the airbag. After the airbag shrinks, it can be smoothly pulled out to obtain a prefabricated tube.

[0053] Then put the prefabricated tube into the preforming mold, the mold temperature is 30℃, the mold is closed and slowly pressurized to 3MPa, and maintained for 10 minutes. During this period, the mold can be opened 2-3 times and pressurized again, which is conducive to removing the air remaining inside the material and improving the density of the composite leaf spring. After this operation, a leaf spring prefabricated part is obtained.

[0054] Finally, the preform is placed in the molding mold, the mold temperature is 120℃, the mold is closed and pressurized to 10MPa, and maintained for 30 minutes, and the resin completes the curing process. After demoulding, it is placed in an oven and post-cured at 150℃-180℃ for 2h to obtain a leaf spring blank. Use sandpaper to grind and remove the flash. If necessary, use a cutting tool to cut off the excess parts at both ends of the leaf spring. Finally, the finished composite leaf spring is obtained, such as Figure 3 shown.

[0055] The variable thickness and cross-section composite leaf spring manufactured by the above method has an experimental bending failure load of 70kN, a torsional moment of 61N·m, and a fatigue life of 2.3 million times. The laying time of a single prepreg is only 30min, which is 90% less than the traditional prepreg manual layer-by-layer laying method, greatly improving production efficiency and reducing manufacturing costs, meeting the requirements of large-scale mass production applications in the automotive industry.

[0056] Example 3

[0057] Different from the embodiment, the prepreg composite material with a fiber angle of 0° is first wound on the surface of the core material, and when the winding thickness reaches more than 25 mm, the prepreg composite material with a fiber angle of 45° is continued to be wound, the temperature of the tube winding machine table is 40°C, and the pressing force is 3MPa. Then the prefabricated tube is placed in the preforming mold, the mold temperature is 50°C, the mold is closed and slowly pressurized to 5MPa, and maintained for 10 minutes.

[0058] Finally, the preform is placed in the molding mold, the mold temperature is 120℃, the mold is closed and pressurized to 12MPa, and maintained for 30 minutes, and the resin completes the curing process. After demoulding, it is placed in an oven and post-cured at 150℃-180℃ for 2h to obtain a leaf spring blank. The flash is polished and removed with sandpaper, and the excess parts at both ends of the leaf spring are cut off with a cutting tool if necessary. Finally, the finished composite leaf spring is obtained.

[0059] The composite leaf springs of equal thickness and cross-section manufactured by the above method have experimentally tested a bending failure load of 75kN, a torsional load of 80N·m, a fatigue life of 3 million times without damage, and a single prepreg laying time of 30min, which is 90% less than the traditional prepreg manual layer-by-layer laying method, greatly improving production efficiency and reducing manufacturing costs, meeting the requirements of large-scale mass production applications in the automotive industry.

[0060] Comparative Example 1

[0061] In order to better illustrate the advantages of the present invention, the following steps are used to compare the composite leaf spring manufactured by the traditional method of manually stacking prepreg layer by layer and compression molding:

[0062] First, cut the prepreg. Use an automatic cloth cutting machine to cut the unidirectional glass fiber prepreg into rectangular sheets, with a total of 240 sheets, including 150 sheets with the length direction of the sheet being the 0° direction of the fiber, with a size of 1200mm*70mm; and 90 sheets with the length direction of the sheet being the 90° direction of the fiber, with a size of 1200mm*70mm. The cutting time takes 50-60 minutes.

[0063] Then the prepreg is laid out layer by layer manually to make prefabricated parts. According to the ply design requirements, the prepreg is laid out layer by layer on the preforming mold. Each layer is compacted with a roller, scraper and other auxiliary tools to prevent bubbles or other impurities from remaining. In order to ensure the quality of the ply, the preforming mold is closed and slowly pressurized to 3MPa for 3 minutes after every 50 layers. This is repeated until all the prepreg is laid out. It takes 5-6 hours in total.

[0064] Finally, the preform is placed in the molding mold, the mold temperature is 120℃, the mold is closed and pressurized to 10MPa, and maintained for 30 minutes, and the resin completes the curing process. After demoulding, it is placed in an oven and post-cured at 150-180℃ for 2 hours to obtain a leaf spring blank. Use sandpaper to grind and remove the flash, and use a cutting tool to cut off the excess parts at both ends of the leaf spring if necessary. Finally, the finished composite leaf spring is obtained.

[0065] The composite leaf springs of equal thickness and cross-section manufactured by the above method have an experimental test bending failure load of 50kN, a torsional moment of 43N·m, and a fatigue load life of 1.3 million times.

[0066] The preferred embodiments of the present invention have been described in detail above, but it should be understood that after reading the above teachings of the present invention, those skilled in the art may make various changes or modifications to the present invention. These equivalent forms also fall within the scope defined by the appended claims of this application.

Claims

1. A method for preparing a composite leaf spring, characterized in that: include: (1) Winding and pressing the prepreg on the surface of the core material, and then extracting the core material to obtain a prefabricated tube; (2) placing the prefabricated tube into a preforming mold, and applying pressure to the mold at room temperature, wherein the pressure is 2-5 MPa, to obtain a prefabricated part; (3) placing the preform into a molding die, applying pressure, and demolding to obtain a composite leaf spring; The fiber angle of the prepreg is 0°-135°, and the fiber angle is the angle between the length direction of the prepreg fiber after winding and the length direction of the composite leaf spring; The core material surface is wound with prepreg, comprising: First, the prepreg with a fiber angle of 0° is wound on the surface of the core material. When the winding thickness reaches more than 10 mm, the prepreg with a fiber angle of any angle between 0° and 135° is continued to be wound.

2. The method for preparing a composite leaf spring according to claim 1, characterized in that: The prepreg is a unidirectional woven glass fiber prepreg, wherein the resin mass content is 30%-40% and the single layer thickness is 0.15 mm-0.3 mm.

3. The method for preparing a composite leaf spring according to claim 1, characterized in that: The shape of the prepreg is square, rectangular, trapezoidal or triangular.

4. The method for preparing a composite leaf spring according to claim 1, characterized in that: A tube reel with a table top made of soft material is used to wind and compress the prepreg layer by layer on the surface of the core material. The pressing force is 1 MPa-3 MPa, and the table top temperature is 25°C-40°C.

5. The method for preparing a composite leaf spring according to claim 4, characterized in that: The table top is covered with 5-10 mm of polyurethane or silicone rubber.

6. The method for preparing a composite leaf spring according to claim 1, characterized in that: The core material has a diameter of 10 mm to 30 mm and a length 200 mm to 500 mm longer than the composite leaf spring.

7. The method for preparing a composite leaf spring according to claim 1, characterized in that: The core material is a cylindrical air bag, one end of which is connected to an air inlet valve and the other end is connected to an air outlet valve. The core material is filled with gas.