A corrosion-resistant aluminum alloy plate and its processing technology
By forming a composite base film and a DLC film layer on the aluminum alloy plate, the problem that the existing aluminum alloy surface modification process cannot improve the wear resistance and corrosion resistance is solved, and the wear resistance and corrosion resistance of the aluminum alloy plate are improved. Significant improvement.
Patent Information
- Application Number
- CN202211599278.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The existing aluminum alloy surface modification process cannot effectively improve its wear resistance and corrosion resistance, and cannot meet actual needs.
After ultrasonic cleaning with absolute ethanol and deionized water, cleaning with argon ions, and co-sputtering with ceria target, aluminum target, titanium target, and chromium target to form a composite bottom film, and then ion nitriding treatment is performed, and finally A DLC film is deposited on the surface of the aluminum alloy substrate to improve its bonding strength and wear resistance.
Significantly improve the wear resistance and corrosion resistance of aluminum alloy plates, enhance their mechanical properties and surface hardness, and form corrosion-resistant aluminum alloy plates with high practicality.
Smart Images

Figure BDA0003994555320000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy plates, in particular to a corrosion-resistant aluminum alloy plate and a processing technology thereof. Background Art
[0002] Aluminum alloys generally add one or more alloying elements (such as Cu, Zn, Mg) and some trace elements to pure aluminum to change its composition and organizational structure, so that it has excellent mechanical strength and corrosion resistance, and excellent processing and forming properties. Therefore, compared with other publicly available alloy materials, aluminum alloys have gradually become the preferred processing material for industrial products and are widely used in aerospace, shipping, automobiles, construction and other fields.
[0003] Since aluminum alloy itself has low mechanical strength and poor wear resistance, existing R&D personnel will perform surface modification on it, using processes such as anodizing, thermal spraying, laser cladding, and electroplating to improve the surface wear resistance and corrosion resistance of aluminum alloy products. The deposition of diamond-like carbon film (DLC film) is also a commonly used modification method. However, the products obtained by the existing process still cannot meet our actual needs.
[0004] Therefore, the present application discloses a corrosion-resistant aluminum alloy plate and a processing technology thereof to solve the technical problem. Summary of the invention
[0005] The object of the present invention is to provide a corrosion-resistant aluminum alloy plate and a processing technology thereof to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0008] (1) An aluminum alloy substrate is taken, the surface is polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 10 to 20 minutes in sequence. After drying, the surface is cleaned with argon ions for 5 to 10 minutes, and then a cerium dioxide target, an aluminum target, a titanium target, and a chromium target are co-sputtered to deposit a base film;
[0009] (2) performing ion nitriding treatment on the surface of the base film;
[0010] (3) Taking the aluminum alloy substrate treated in step (2), depositing a DLC film on the surface, ultrasonically cleaning with deionized water, and vacuum drying to obtain a finished product.
[0011] In a more optimized solution, in step (1), the specific steps of co-sputtering are:
[0012] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 0.5-1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 1500-2000 W, and the power of the aluminum-palladium target is 300-500 W. Sputter for 10-20 minutes.
[0013] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 100-200W, the aluminum palladium power is adjusted to 150-200W, and continue sputtering for 5-10 minutes;
[0014] S3: Repeat steps S1 to S2 2 to 3 times, and turn off the cerium dioxide palladium;
[0015] S4: Turn on the titanium target and chromium target, with the power of the chromium target at 1500-2000W, the power of the titanium target at 1000-1200W, and the power of the aluminum-palladium target at 300-500W. Sputter with the titanium target, aluminum-palladium target and chromium target for 40-50 minutes, then turn off the target to form a base film.
[0016] In the more optimized solution, in step (3), the DLC film deposition process parameters are: acetylene flow rate is 50-60 mL / min, argon flow rate is 20-30 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 100-120°C, the ion source power is 4-5 kW, and the deposition time is 2-3 h.
[0017] In a more optimized solution, in step (2), the ion nitriding temperature is 460-480°C, the nitriding time is 4-6 hours, and the nitriding pressure is 0.6-0.8 Pa.
[0018] In a more optimized solution, in step (2), during ion nitriding, sponge titanium and ferroboron mixture are placed around the aluminum alloy substrate to achieve titanium-boron-nitrogen composite nitriding.
[0019] The most optimized solution is 1mm around the aluminum alloy substrate 2 8 to 10 mg of the mixture is placed per unit area, and the mass ratio of sponge titanium to ferroboron in the mixture is 3:1.
[0020] In a more optimized solution, in step (1), the contents of the components of the aluminum alloy substrate are as follows: by mass fraction, Zn: 5.85-6.42%, Mg: 2.2-2.3%, Cu: 2.13-2.18%, Fe: 0.05-0.055%, Si: 0.02-0.041%, Mn: 0.01-0.019%, Zr: 0.094-0.12%, Cr: 0.003-0.01%, and the remainder is Al and unavoidable impurities.
[0021] A more optimized solution is an aluminum alloy sheet obtained by processing according to any one of the processing techniques for corrosion-resistant aluminum alloy sheets described above.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] The invention discloses a corrosion-resistant aluminum alloy plate and a processing technology thereof. The scheme uses an aluminum alloy substrate as a substrate and performs sputtering deposition of a film layer on the surface of the substrate to improve the corrosion resistance and wear resistance of the aluminum alloy plate. The contents of the components of the aluminum alloy substrate are as follows: by mass fraction, Zn: 5.85-6.42%, Mg: 2.2-2.3%, Cu: 2.13-2.18%, Fe: 0.05-0.055%, Si: 0.02-0.041%, Mn: 0.01-0.019%, Zr: 0.094-0.12%, Cr: 0.003-0.01%, and the remainder is Al and unavoidable impurities. The aluminum alloy substrate formed by processing with the formula has relatively excellent mechanical properties and can be suitable for implementation of the scheme.
[0024] On this basis, the scheme first polishes the surface of the aluminum alloy substrate with sandpaper, washes it with anhydrous ethanol and deionized water, and then washes it with argon ions, and then co-sputters with cerium dioxide target, aluminum target, titanium target, and chromium target as target materials to deposit and form a base film; during sputtering deposition, the present application designs the scheme as "chromium target and aluminum palladium are pre-sputtered to form a base layer, aluminum palladium and cerium dioxide palladium are sputtered to form a transition film, and then titanium target, aluminum palladium and chromium target are co-sputtered" to form a composite base film. The technical effect achieved is: since the outermost layer of the aluminum alloy sheet is a hard DLC film layer, and the hardness of the aluminum alloy substrate is relatively low, the base film, as a transition layer between the two, can provide support for the outer DLC film, which can not only improve the bonding strength between the aluminum alloy substrate and the DLC film layer, but also improve the bearing capacity and surface wear resistance of the aluminum alloy sheet.
[0025] It should be emphasized here: the present application creatively limits the sputtering order of each target material and constructs a composite base film therefrom. Compared with a single titanium film or chromium film, the bonding strength between the DLC film and the aluminum-aluminum alloy substrate is more significantly improved, and the surface wear resistance of the aluminum alloy plate is also improved.
[0026] At the same time, after the sputtering of the base film, the present solution performs an ion nitriding treatment step, the purpose of which is to promote the formation of aluminum-based intermetallic compounds, on the one hand, to improve the surface hardness of the base film, thereby improving its bearing capacity and improving its bonding strength with the outer DLC film layer, on the other hand, after ion nitriding, the overall density of the base film is increased, and the grains are refined and the size is more uniform. As a physical barrier, it can effectively hinder the entry of corrosive media, thereby improving the corrosion resistance of the aluminum alloy sheet. The scheme here also provides other embodiments, such as introducing boron and titanium to achieve boron-titanium-nitrogen co-diffusion. The present solution ion nitrides on the surface of the aluminum alloy, so its temperature should be lower than the overburning temperature of the aluminum alloy to avoid excessive grain coarsening, which is limited to "460-480°C". Under low temperature conditions, the introduction of boron and titanium can promote the diffusion efficiency and optimize the diffusion effect, thereby improving the bonding performance between the base film and the aluminum alloy substrate.
[0027] On this basis, the plan deposits a DLC film on the outermost side of the aluminum alloy substrate, and limits the process parameters as follows: acetylene flow rate is 50-60mL / min, argon flow rate is 20-30mL / min, the pressure in the chamber is controlled to be 2.0Pa, the substrate temperature is 100-120°C, the ion source power is 4-5kW, and the deposition time is 2-3h. The DLC film has the characteristics of high hardness, wear resistance, friction reduction, lubrication and corrosion resistance, which can effectively guarantee the comprehensive performance of the aluminum alloy plate; and due to the presence of the composite base film and ion nitriding steps, the bonding strength between the DLC film and the aluminum alloy substrate is high, and the wear resistance is further improved.
[0028] The present application discloses a corrosion-resistant aluminum alloy plate and a processing technology thereof. The overall process design is reasonable. By limiting the sputtering sequence of the target material to deposit and form a composite base film, and then performing DLC film deposition after ion nitriding, the prepared aluminum alloy plate has excellent corrosion resistance, high surface hardness, excellent wear resistance, and high practicality. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In this embodiment, the contents of the components of the aluminum alloy substrate are: by mass fraction, Zn: 5.85%, Mg: 2.28%, Cu: 2.13%, Fe: 0.055%, Si: 0.041%, Mn: 0.019%, Zr: 0.094%, Cr: 0.003%, and the remainder is Al and unavoidable impurities.
[0031] The titanium target, aluminum palladium and chromium target are pure titanium, pure aluminum and pure chromium; the particle size of sponge titanium is 3-5 mm; the chemical composition of ferroboron is as follows by mass fraction: B: 17.51%, Al: 0.023%, Si: 0.23%, P: 0.031%, C: 0.20%, S: 0.003%, and the balance is iron.
[0032] Embodiment 1:
[0033] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0034] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 10 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then co-sputtered with a cerium dioxide target, an aluminum target, a titanium target, and a chromium target to deposit a base film;
[0035] The specific steps of co-sputtering are:
[0036] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 2000 W, and the power of the aluminum-palladium target is 300 W. Sputtering is performed for 10 minutes.
[0037] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 200W, the aluminum palladium power is adjusted to 150W, and continue sputtering for 5 minutes;
[0038] S3: Repeat steps S1 to S2 for 3 times, and turn off the cerium dioxide palladium;
[0039] S4: Turn on the titanium target and chromium target, the chromium target power is 2000W, the titanium target power is 1200W, and the aluminum palladium power is adjusted to 400W. Sputter with the titanium target, aluminum palladium and chromium target for 40 minutes, turn off the target material, and form a base film.
[0040] (2) Perform ion nitriding treatment on the surface of the base film; the ion nitriding temperature is 480°C, the nitriding time is 4h, and the nitriding pressure is 0.8Pa.
[0041] (3) Take the aluminum alloy substrate treated in step (2), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 100°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning, and vacuum drying to obtain a finished product.
[0042] Embodiment 2:
[0043] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0044] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 15 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then co-sputtered with a cerium dioxide target, an aluminum target, a titanium target, and a chromium target to deposit a base film;
[0045] The specific steps of co-sputtering are:
[0046] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 2000 W, and the power of the aluminum-palladium target is 300 W. Sputtering is performed for 15 minutes.
[0047] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 200W, the aluminum palladium power is adjusted to 150W, and continue sputtering for 10 minutes;
[0048] S3: Repeat steps S1 to S2 for 3 times, and turn off the cerium dioxide palladium;
[0049] S4: Turn on the titanium target and chromium target, the chromium target power is 2000W, the titanium target power is 1200W, and the aluminum palladium power is adjusted to 400W. Sputter with the titanium target, aluminum palladium and chromium target for 45 minutes, turn off the target material, and form a base film.
[0050] (2) Perform ion nitriding treatment on the surface of the base film; the ion nitriding temperature is 480°C, the nitriding time is 5 hours, and the nitriding pressure is 0.8 Pa.
[0051] (3) Take the aluminum alloy substrate treated in step (2), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 120°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning, and vacuum drying to obtain a finished product.
[0052] Embodiment 3:
[0053] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0054] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 20 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then co-sputtered with a cerium dioxide target, an aluminum target, a titanium target, and a chromium target to deposit a base film;
[0055] The specific steps of co-sputtering are:
[0056] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 2000 W, and the power of the aluminum-palladium target is 300 W. The sputtering is carried out for 20 minutes.
[0057] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 200W, the aluminum palladium power is adjusted to 150W, and continue sputtering for 10 minutes;
[0058] S3: Repeat steps S1 to S2 for 3 times, and turn off the cerium dioxide palladium;
[0059] S4: Turn on the titanium target and chromium target, the chromium target power is 2000W, the titanium target power is 1200W, and the aluminum palladium power is adjusted to 400W. Sputter with the titanium target, aluminum palladium, and chromium target for 50 minutes, turn off the target material, and form a base film.
[0060] (2) Perform ion nitriding treatment on the surface of the base film; the ion nitriding temperature is 480°C, the nitriding time is 6 hours, and the nitriding pressure is 0.8 Pa.
[0061] (3) Take the aluminum alloy substrate treated in step (2), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 120°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning, and vacuum drying to obtain a finished product.
[0062] Example 4: Introducing boron and titanium during ion nitriding.
[0063] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0064] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 15 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then co-sputtered with a cerium dioxide target, an aluminum target, a titanium target, and a chromium target to deposit a base film;
[0065] The specific steps of co-sputtering are:
[0066] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 2000 W, and the power of the aluminum-palladium target is 300 W. Sputtering is performed for 15 minutes.
[0067] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 200W, the aluminum palladium power is adjusted to 150W, and continue sputtering for 10 minutes;
[0068] S3: Repeat steps S1 to S2 for 3 times, and turn off the cerium dioxide palladium;
[0069] S4: Turn on the titanium target and chromium target, the chromium target power is 2000W, the titanium target power is 1200W, and the aluminum palladium power is adjusted to 400W. Sputter with the titanium target, aluminum palladium and chromium target for 45 minutes, turn off the target material, and form a base film.
[0070] (2) Ion nitriding treatment is performed on the surface of the base film; the ion nitriding temperature is 480°C, the nitriding time is 5 hours, and the nitriding pressure is 0.8 Pa. During ion nitriding, titanium sponge and boron iron mixture are placed around the aluminum alloy substrate to achieve titanium boron nitrogen composite nitriding. 2 10 mg of the mixture is placed per unit area, and the mass ratio of sponge titanium and ferroboron in the mixture is 3:1.
[0071] (3) Take the aluminum alloy substrate treated in step (2), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 120°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning, and vacuum drying to obtain a finished product.
[0072] Comparative Example 1:
[0073] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0074] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 15 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then co-sputtered with a cerium dioxide target, an aluminum target, a titanium target, and a chromium target to deposit a base film;
[0075] The specific steps of co-sputtering are:
[0076] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 2000 W, and the power of the aluminum-palladium target is 300 W. Sputtering is performed for 15 minutes.
[0077] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 200W, the aluminum palladium power is adjusted to 150W, and continue sputtering for 10 minutes;
[0078] S3: Repeat steps S1 to S2 for 3 times, and turn off the cerium dioxide palladium;
[0079] S4: Turn on the titanium target and chromium target, the power of the chromium target is 2000W, the power of the chromium target and the titanium target is 1200W, and the power of the aluminum palladium target is adjusted to 400W. Sputter with the titanium target, aluminum palladium and chromium target for 45 minutes, turn off the target material, and form a base film.
[0080] (2) Take the aluminum alloy substrate treated in step (1), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 120°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning is performed, and vacuum drying is performed to obtain a finished product.
[0081] Example 2 was used as a control group. In Comparative Example 1, ion nitriding treatment was not performed, and the other processes remained unchanged.
[0082] Comparative Example 2:
[0083] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0084] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 15 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then co-sputtered with a cerium dioxide target, an aluminum target, and a chromium target to deposit a base film;
[0085] The specific steps of co-sputtering are:
[0086] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 2000 W, and the power of the aluminum-palladium target is 300 W. Sputtering is performed for 15 minutes.
[0087] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 200W, the aluminum palladium power is adjusted to 150W, and continue sputtering for 10 minutes;
[0088] S3: Repeat steps S1 to S2 for 3 times, and turn off the cerium dioxide palladium;
[0089] S4: Turn on the chromium target, the chromium target power is 2000W, the aluminum palladium power is adjusted to 400W, and the aluminum palladium and chromium targets are sputtered for 45 minutes. Then the target is turned off to form a base film.
[0090] (2) Perform ion nitriding treatment on the surface of the base film; the ion nitriding temperature is 480°C, the nitriding time is 5 hours, and the nitriding pressure is 0.8 Pa.
[0091] (3) Take the aluminum alloy substrate treated in step (2), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 120°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning, and vacuum drying to obtain a finished product.
[0092] Example 2 was used as a control group. No titanium target was introduced in Example 2, and the other processes remained unchanged.
[0093] Comparative Example 3:
[0094] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0095] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 15 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then a base film was deposited by magnetron sputtering with a chromium target;
[0096] The specific steps of co-sputtering are: introduce argon gas into the chamber to maintain the chamber pressure at 1.0Pa, first turn on the chromium target with a power of 2000W and sputter for 90min; then close the target to form a base film.
[0097] (2) Perform ion nitriding treatment on the surface of the base film; the ion nitriding temperature is 480°C, the nitriding time is 5 hours, and the nitriding pressure is 0.8 Pa.
[0098] (3) Take the aluminum alloy substrate treated in step (2), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 120°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning, and vacuum drying to obtain a finished product.
[0099] Example 2 was used as the control group. In Comparative Example 3, aluminum palladium, cerium dioxide palladium and titanium targets were not introduced, and only chromium target sputtering was used, and the other processes remained unchanged.
[0100] Comparative Example 4:
[0101] A processing technology for a corrosion-resistant aluminum alloy plate comprises the following steps:
[0102] (1) An aluminum alloy substrate was taken, the surface was polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 15 minutes in sequence. After drying, the surface was cleaned with argon ions for 10 minutes, and then co-sputtered with a cerium dioxide target, an aluminum target, a titanium target, and a chromium target to deposit a base film;
[0103] The specific steps of co-sputtering are:
[0104] S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 2000 W, and the power of the aluminum-palladium target is 300 W. Sputtering is performed for 15 minutes.
[0105] S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 200W, the aluminum palladium power is adjusted to 150W, and continue sputtering for 10 minutes;
[0106] S3: Repeat steps S1 to S2 for 3 times, and turn off the cerium dioxide palladium;
[0107] S4: Turn on the titanium target and chromium target, the chromium target power is 2000W, the titanium target power is 1200W, and the aluminum palladium power is adjusted to 400W. Sputter with the titanium target, aluminum palladium and chromium target for 45 minutes, turn off the target material, and form a base film.
[0108] (2) Ion nitriding treatment is performed on the surface of the base film; the ion nitriding temperature is 480°C, the nitriding time is 5 hours, and the nitriding pressure is 0.8 Pa. During ion nitriding, titanium sponge and boron iron mixture are placed around the aluminum alloy substrate to achieve titanium boron nitrogen composite nitriding. 2 10 mg of the mixture is placed per unit area, and the mass ratio of sponge titanium and ferroboron in the mixture is 3:1.
[0109] (3) Take the aluminum alloy substrate treated in step (2), and deposit a DLC film on the surface. The DLC film deposition process parameters are: acetylene flow rate is 60 mL / min, argon flow rate is 20 mL / min, the pressure in the chamber is controlled to be 2.0 Pa, the substrate temperature is 120°C, the ion source power is 4 kW, the deposition time is 3 h, deionized water ultrasonic cleaning, and vacuum drying to obtain a finished product.
[0110] Example 4 is used as the control group, and the 1 mm 2 4 mg of the mixture is placed per unit area, and the mass ratio of sponge titanium to ferroboron is 1:1.
[0111] Detection experiment:
[0112] 1. The aluminum alloy plates prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were used to test the bonding strength of the DLC film on the surface of the aluminum alloy substrate by the scratch method. The test was conducted using a Rockwell C conical diamond indenter, model AB228, with a cone angle of 120° and a tip radius of 0.2 μm. During the test, the progressive normal load was 0 to 15 N, the scratch length was 3 mm, and the scratch speed was 1.5 mm / min. The bonding strength was characterized by the critical load at which the coating was completely peeled off.
[0113] 2. Take the aluminum alloy plates prepared in Examples 1 to 4 and Comparative Examples 1 to 4 and conduct friction and wear tests. The test temperature is 25°C, the humidity is 60%, the friction pair is a GCr15 steel ball with a diameter of 6 mm, the sliding frequency is 5 Hz, and the single sliding stroke is 5 mm. The friction time is 30 min and the load is 5 N. Measure and calculate the wear rate.
[0114] 3. Take the aluminum alloy plates prepared in Examples 1 to 4 and Comparative Examples 1 to 4, and test the corrosion resistance according to the "Neutral Salt Spray Test (NSS) Method for Abrasion Resistance of Metal Coatings and Chemical Treatment Layers of Light Industrial Products" disclosed in GB / T5938-86. After the test, the corrosion resistance grade is evaluated according to GB / T5944-86.
[0115]
[0116] Conclusion: The overall process design of this application is reasonable. By limiting the sputtering sequence of the target material to deposit and form a composite base film, and then performing DLC film deposition after ion nitriding, the prepared aluminum alloy plate has excellent corrosion resistance, high surface hardness, excellent wear resistance, and high practicality.
[0117] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A processing technology for corrosion-resistant aluminum alloy sheet, Features: The following steps are involved: (1) An aluminum alloy substrate is taken, the surface is polished with sandpaper, and ultrasonically cleaned with anhydrous ethanol and deionized water for 10 to 20 minutes in sequence. After drying, the surface is cleaned with argon ions for 5 to 10 minutes, and then a cerium dioxide target, an aluminum target, a titanium target, and a chromium target are co-sputtered to deposit a base film; In step (1), the specific steps of co-sputtering are: S1: Argon gas is introduced into the chamber to maintain the chamber pressure at 0.5-1.0 Pa. The chromium target and aluminum target are first turned on. The power of the chromium target is 1500-2000 W, and the power of the aluminum-palladium target is 300-500 W. Sputter for 10-20 minutes. S2: Turn off the chromium target, turn on the ceria palladium, the ceria palladium power is 100-200W, the aluminum palladium power is adjusted to 150-200W, and continue sputtering for 5-10 minutes; S3: Repeat steps S1 to S2 2 to 3 times, and turn off the cerium dioxide palladium; S4: Turn on the titanium target and the chromium target, the power of the chromium target is 1500-2000W, the power of the titanium target is 1000-1200W, the power of the aluminum palladium is adjusted to 300-500W, and the titanium target, aluminum palladium and chromium target are sputtered for 40-50 minutes, and the target is turned off to form a base film; The content of each component of the aluminum alloy substrate is: by mass fraction, Zn: 5.85-6.42%, Mg: 2.2-2.3%, Cu: 2.13-2.18%, Fe: 0.05-0.055%, Si: 0.02-0.041%, Mn: 0.01-0.019%, Zr: 0.094-0.12%, Cr: 0.003-0.01%, and the balance is Al and unavoidable impurities; (2) performing ion nitriding treatment on the surface of the base film; (3) Taking the aluminum alloy substrate treated in step (2), depositing a DLC film on the surface, ultrasonically cleaning with deionized water, and vacuum drying to obtain a finished product.
2. A processing technology for a corrosion-resistant aluminum alloy sheet according to claim 1, Features: In step (3), the DLC film deposition process parameters are: acetylene flow rate is 50-60 mL / min, argon flow rate is 20-30 mL / min, the pressure in the control chamber is 2.0 Pa, the substrate temperature is 100-120°C, the ion source power is 4-5 kW, and the deposition time is 2-3 h.
3. The processing technology of the corrosion-resistant aluminum alloy sheet according to claim 1, Features: In step (2), the ion nitriding temperature is 460-480° C., the nitriding time is 4-6 hours, and the nitriding pressure is 0.6-0.8 Pa.
4. A processing technology for a corrosion-resistant aluminum alloy sheet according to claim 3, Features: In step (2), during ion nitriding, sponge titanium and ferroboron mixture are placed around the aluminum alloy substrate to achieve titanium-boron-nitrogen composite nitriding.
5. A processing technology for a corrosion-resistant aluminum alloy sheet according to claim 4, Features: 1mm around aluminum alloy substrate 2 8 to 10 mg of the mixture is placed per unit area, and the mass ratio of sponge titanium to ferroboron in the mixture is 3:
1.
6. An aluminum alloy sheet obtained by processing according to the processing technology of a corrosion-resistant aluminum alloy sheet according to any one of claims 1 to 5.