A method for improving the anti-breakage performance of cemented carbide coated tools and cemented carbide coated tools
By pressurized heat treatment and chemical vapor deposition on cemented carbide substrate, the crack problem caused by the difference in expansion coefficient during cooling of cemented carbide coating tools is solved, and the anti-collapse is significantly improved Performance and service life.
Patent Information
- Application Number
- CN202411245652.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-06
AI Technical Summary
During the cooling process, the tensile stress caused by the difference in the expansion coefficients of the substrate and the coating material in the existing cemented carbide coated tools leads to microcracks in the coating, which reduces the tool's anti-collapse performance.
Use cemented carbide substrates with pores for pressurized heat treatment to eliminate pores and residual stress of the substrate, reduce the tensile stress of the coating, and form composite coatings such as TiN, TiCN and Al2O3 through chemical vapor deposition to ensure the coating density and adhesion.
It effectively avoids the occurrence of thermal cracks on the coating, improves the anti-collapse performance of the tool, and enhances the stability and service life of the product.
Smart Images

Figure CN118756113B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of cemented carbide tools, and in particular relates to a method for improving the anti-breakage performance of a cemented carbide coating tool and a cemented carbide coating tool. Background Art
[0002] The damage of cemented carbide tool coating includes two forms: wear (flank wear, rake face crater, boundary damage, micro-chipping, etc.) and breakage (chipping, flaking, breaking, plastic deformation). The damage is generally restricted by the tool material (including substrate and coating), tool shape and processing conditions.
[0003] Existing CVD (chemical vapor deposition) coated tools deposit coating materials on a cemented carbide substrate. Due to the difference in expansion coefficients between the cemented carbide substrate and the coating material, the coating will produce tensile stress during the cooling process after coating, causing microcracks in the coating. The cracks will greatly reduce the tool material's resistance to breakage.
[0004] CN105506622A discloses a composite coating tool and a manufacturing method thereof. The invention provides a base material and a composite coating on the blade. The composite coating is composed of a tin layer, a titanium carbonitride layer, an intermediate layer, an aluminum oxide layer, and an outermost layer from the inside to the outside. The coated tool is manufactured by CVD (chemical vapor deposition). Compared with a single coating, the invention has a higher bonding strength between the coating and the substrate, which can effectively reduce cutting friction, reduce cutting force and cutting temperature, reduce tool wear, inhibit the generation of thermal cracks, and effectively prevent the coating layer from flaking off; the coated tool better solves the contradiction between tool strength and toughness, and greatly improves the tool's durability and cutting speed. This scheme mainly starts from the setting direction of the composite coating to enhance the bonding strength between the coating and the substrate. However, it does not consider the impact of stress on the material, such as elastic deformation, plastic deformation, and damage.
[0005] CN105401129A discloses a superhard composite coating and a preparation method thereof, wherein a multi-layer coating is arranged on a superhard base material, and the coating is sequentially composed of a titanium layer, an intermediate layer, an aluminum oxide layer, and a surface layer from the inside to the outside, and the coating is made by CVD (chemical vapor deposition). This solution can inhibit the generation of thermal cracks and effectively prevent the coating layer from flaking off. However, it does not consider the effect of the residual stress release of the material after cooling on the entire tool, so there is a risk of thermal cracks in the coating.
[0006] In summary, it is very necessary to invent a solution that fully considers the relaxation of material stress to effectively improve the anti-breakage performance of cemented carbide coated tools. This can ensure the stability and life of the tool products, greatly improve the safety of use, and has great practical significance and market value. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present invention provides a method for improving the anti-breakage performance of cemented carbide coated cutting tools. A cemented carbide substrate with pores is used as the substrate to be coated, and then coating is performed layer by layer on the substrate. In order to eliminate the pores and release the residual stress of the substrate, a pressurized heat treatment method is adopted to ensure the density of the substrate while avoiding the generation of thermal cracks in the coating, thereby improving the anti-breakage performance of the entire product.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] Disclosed is a method for improving the anti-breakage performance of a cemented carbide coated tool. The method comprises the following steps: adjusting the relative density of a cemented carbide substrate layer according to the difference in expansion coefficients between the cemented carbide substrate layer and a coating material, wherein the relative density of the cemented carbide substrate layer is 95.5%-99.5%, so that pores exist in the cemented carbide substrate layer; heat treatment is performed on the coated cemented carbide coated tool to increase the shrinkage of the cemented carbide substrate layer; and cooling is performed after the heat treatment to eliminate the pores in the cemented carbide substrate layer, reduce the tensile stress of the cemented carbide substrate layer or change the compressive stress, and alleviate the generation of cracks in the coating.
[0010] The method of improving the anti-breakage performance of cemented carbide coated cutting tools of the present invention breaks the inherent thinking of conventional technology, that is, the cemented carbide substrate layer has a relative density of 100%, ensuring good strength and anti-breakage performance. However, after the coating is cooled, the expansion coefficient of the substrate is smaller than that of the coating, which will cause tensile stress in the coating. After rapid cooling, thermal cracks and residual tensile stress will be generated, which will affect the anti-breakage performance of the cutting tool.
[0011] If a tool is prepared using a porous substrate, the tool prepared using conventional technology will have its anti-breakage performance deteriorated due to the presence of pores in the substrate. Therefore, the measure taken by the present invention is to perform pressurized heat treatment on the substrate. The pressurized treatment can eliminate the pores. At the same time, due to the volume shrinkage of the substrate after the coating, the amplitude of the matrix expansion coefficient and the coating expansion coefficient will be reduced, so that the tensile stress of the coating is reduced or changed to compressive stress, thereby alleviating the generation of thermal cracks in the coating.
[0012] Furthermore, the coating is a composite coating formed by alternately stacking TiN layers, TiCN layers and Al2O3 layers by chemical vapor deposition, and each layer of the composite coating is added with at least one trace element of Zr, Hf, Cr, Mo, Nb, Ta, Y, Si and W, and the value of the trace element in the molecular formula is between 0.05 and 0.2.
[0013] Furthermore, the total thickness of the composite coating is 10µm~50µm, and the thickness of a single layer is 2µm~30µm.
[0014] Furthermore, the heat treatment process: after the coating is applied, heat treatment is directly carried out at a temperature of 1100°C to 1300°C, Ar gas pressure heat treatment, a pressure of 8MPa to 20MPa, and a treatment time of 2h to 5h. After the heat treatment is completed, the power is turned off and the furnace is cooled to room temperature. After the coating is completed, the pressure in the furnace is increased, and the inside of the blade will be squeezed by the external pressure. At the same time, due to the increase in temperature, the softening temperature is gradually reached, and the grain boundaries of the WC main metallographic phase in the matrix and the added powder produce sliding filling pores, thereby improving the density of the substrate; at the same time, after cooling, the shrinkage of the substrate will be greater than the shrinkage rate of normal process products, thereby achieving the effect of easing the transition of the tensile stress of the coating to the compressive stress.
[0015] Furthermore, the heat treatment process is as follows: after the coating is applied, it is taken out of the furnace and cooled to room temperature, and then put into the pressurized furnace again for heat treatment, the temperature is raised to 1150℃~1350℃, Ar gas pressurized heat treatment, the treatment pressure is 8MPa~20MPa, and the treatment time is 2h~5h. If it is not possible to perform pressurized heat treatment continuously, it can be put into the pressurized furnace again for heat treatment after the coating is applied and the furnace is cooled. Since the softening temperature of the substrate will lag slightly, the pressurized heat treatment can be performed at a higher temperature. After the heat treatment is completed, the power is turned off and the furnace is cooled to room temperature.
[0016] Furthermore, the cemented carbide substrate layer includes refractory metal hard compound powder, bonding metal powder and compound powder of other metal components. By weight, the content of the refractory metal hard compound is 80%~95%, the content of the bonding metal powder is 5%~15%, and the compound powder of other metal components is 0%~15%.
[0017] Furthermore, the refractory metal hard compound powder is WC powder, the bonding metal powder is at least one of Co powder and Ni powder, and the compound powder of other metal components is at least one compound powder of Ti, Zr, Hf, Cr, Mo, Nb, Ta, Y and Si metal components.
[0018] Furthermore, the specific steps of the chemical vapor deposition method include:
[0019] S1. Forming a bottom TiN layer: Based on a total volume fraction of 100 vol%, the first reaction gas is a mixture of 2 vol% to 8 vol% TiCl4 gas, 15 vol% to 65 vol% N2 gas and the remainder H2 gas, the temperature is set to 750°C to 950°C, and the bottom TiN layer is formed for 30 min to 120 min under the atmosphere of the first reaction gas at 30 kPa to 50 kPa;
[0020] S2. MT-TiCN layer formation: based on a total volume fraction of 100 vol%, the second reaction gas is a mixture of 2 vol% to 10 vol% TiCl4 gas, 15 vol% to 65 vol% N2 gas, 1 vol% to 3 vol% CH3CN gas and the remainder H2 gas. Under the atmosphere of the second reaction gas, the temperature is set to 750°C to 850°C, and the MT-TiCN layer is formed at 5 kPa to 25 kPa for 300 min to 900 min.
[0021] S3. Intermediate TiCN layer film formation: Based on the total volume fraction of 100 vol%, the third reaction gas is a mixture of 10 vol% to 30 vol% TiCl4, 5 vol% to 20 vol% CH4 gas, 5 vol% to 15 vol% N2 gas, 0.5 vol% to 1 vol% CO gas, 0.5 vol% to 3 vol% AlCl3 gas and the remainder H2 gas. In the atmosphere of the third reaction gas, the temperature is set to 900 ° C to 1050 ° C, and the intermediate TiCN layer is formed at 5 kPa to 40 kPa for 5 min to 30 min;
[0022] S4. Forming an Al2O3 layer: First, forming a crystal nucleus of aluminum oxide crystals, and then, based on a total volume fraction of 100 vol%, a fourth reaction gas is composed of 5 vol% to 15 vol% AlCl3 gas, 0.5 vol% to 2.5 vol% HCl gas, 0.5 vol% to 5 vol% CO2 gas, 0 vol% to 1 vol% H2S gas and a remainder of H2 gas. In the atmosphere of the fourth reaction gas, the temperature is set to 950 ° C to 1100 ° C, and the Al2O3 film is formed at 5 kPa to 20 kPa for 400 min to 800 min;
[0023] S5. Forming a TiN layer: Based on a total volume fraction of 100 vol%, the fifth reaction gas is a mixture of 2 vol% to 10 vol% TiCl4 gas, 25 vol% to 60 vol% N2 gas and the remainder H2 gas. Under the atmosphere of the fifth reaction gas, the temperature is set to 960°C to 1100°C, and the film is formed at 30 kPa to 85 kPa for 30 min to 90 min.
[0024] Furthermore, the method for forming the nucleus of aluminum oxide crystals is: based on the total volume fraction of 100 vol%, a mixture of 5 vol% to 15 vol% AlCl3 gas, 0.1 vol% to 1.2 vol% HCl gas, 0.1 vol% to 5.5 vol% CO2 gas and the remainder H2 gas is used, and nucleation is carried out under this gas atmosphere at 950°C to 1050°C, 5 kPa to 10 kPa, and a time of 3 min to 12 min.
[0025] Another object of the present invention is to prepare a cemented carbide coated tool using the above method for improving the anti-breakage performance of cemented carbide coated tools. The coating of the base TiN layer, MT-TiCN layer, intermediate TiCN layer, Al2O3 layer and TiN layer has good density, and the cross section of the coating has no pores and cracks penetrating the coating under an electron microscope at 1000 times.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The method for improving the anti-breakage performance of cemented carbide coated cutting tools provided by the present invention adopts a cemented carbide substrate with pores as the substrate to be coated, and then coats the substrate layer by layer. In order to eliminate the pores and release the residual stress of the substrate, a pressurized heat treatment method is adopted to ensure the density of the substrate while avoiding the generation of thermal cracks in the coating, thereby improving the anti-breakage performance of the entire product. The entire method is highly operable, and the performance of the prepared cemented carbide coated cutting tools in all aspects meets the use requirements, especially the anti-breakage performance has significant advantages over the coated cutting tools prepared by ordinary methods.
[0028] The method for improving the anti-breakage performance of cemented carbide coated tools provided by the present invention comprehensively considers both the substrate and the coating, and performs pressurized heat treatment on the substrate. The pressurized treatment can eliminate pores, and at the same time, due to the volume shrinkage of the substrate after the coating, the difference between the substrate expansion coefficient and the coating expansion coefficient will be reduced, so that the tensile stress of the coating is reduced or changes to compressive stress, and the generation of thermal cracks in the coating is alleviated. A new technical idea is provided for the preparation of coated tools. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A metallographic diagram of a cemented carbide tool material substrate in the method for improving the anti-breakage performance of a cemented carbide coated tool according to the present invention.
[0030] Figure 2 The metallographic diagram of the coating of the cemented carbide tool material in the method for improving the anti-breakage performance of the cemented carbide coated tool according to the present invention.
[0031] Among them, 1-surface layer, 2-aluminum oxide layer, 3-transition layer, 4-TiCN layer, 5-TiN layer. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings. The accompanying drawings are only for illustrative purposes and are only schematic diagrams, not actual pictures, and should not be construed as limiting the present invention. In order to better illustrate the embodiments of the present invention, some parts of the accompanying drawings may be omitted, enlarged or reduced, and do not represent the size of the actual product. It is understandable to those skilled in the art that some well-known structures and their descriptions in the accompanying drawings may be omitted.
[0033] The method for improving the anti-breakage performance of cemented carbide coated cutting tools of the present invention is to adjust the relative density of the cemented carbide substrate layer according to the difference in expansion coefficients between the cemented carbide substrate layer and the coating material, and the relative density of the cemented carbide substrate layer is 95.5% to 99.5%, so that pores exist in the cemented carbide substrate layer; the coated cemented carbide coated cutting tools are heat treated to increase the shrinkage of the cemented carbide substrate layer; and the cemented carbide substrate layer is cooled after the heat treatment to eliminate the pores in the cemented carbide substrate layer, reduce the tensile stress of the cemented carbide substrate layer or change the compressive stress, and alleviate the generation of coating cracks. The specific preparation method is as follows.
[0034] Example 1: The cemented carbide coated tool of this example is prepared using a method for anti-breakage performance. First, prepare the cemented carbide substrate layer. Its preparation method is roughly the same as the general cemented carbide preparation. The cemented carbide coated tool material in this example is prepared at a ratio of 95% WC powder and 5% metal Co powder by weight. The powder is added with 20% to 30% alcohol solvent by weight of the powder, and ball milling and crushing are performed for a specified time of 30h to 50h to form a slurry. Add 2% to 5% paraffin binder by weight of the powder to the slurry, and after further mixing, use a spray drying tower to spray dry to form a mixture.
[0035] Subsequently, after dewaxing by pressing and forming in a cemented carbide sintering furnace, the temperature of the sintering furnace is raised to a firing temperature of 1380°C~1480°C in a reduced pressure environment of 20Pa~200Pa, and the firing is performed for 0.5h~1.0h. The relative density of the blank matrix is strictly controlled to be 95.5%~99.5%, thereby producing a cemented carbide blank blade.
[0036] The carbide blank blade is end-face ground, the edge is passivated, the end face is brushed, and finally cleaned in preparation for coating.
[0037] The prepared cemented carbide blank blade is then subjected to chemical vapor deposition (CVD) to form a film coating on the surface of the substrate. The total thickness of the composite coating is 10µm to 50µm, and the thickness of a single layer is 2µm to 10µm; the thickness of a single layer in this embodiment is 2µm.
[0038] The specific steps include: S1. forming a bottom TiN layer: based on a total volume fraction of 100 vol%, the first reaction gas is a mixture of 2 vol% to 3 vol% TiCl4 gas, 60 vol% to 65 vol% N2 gas and the remainder H2 gas, adjusting the mixed gas and introducing it into the reactor chamber, setting the temperature to 750°C to 850°C, and forming the bottom TiN layer under the atmosphere of the first reaction gas at 30 kPa to 35 kPa for 40 min to 50 min;
[0039] S2. MT-TiCN layer formation: based on a total volume fraction of 100 vol%, the second reaction gas is a mixture of 2 vol% to 4 vol% TiCl4 gas, 60 vol% to 65 vol% N2 gas, 1 vol% to 2 vol% CH3CN gas and the remainder H2 gas. The mixed gas is adjusted and introduced into the reactor chamber. Under the atmosphere of the second reaction gas, the temperature is set to 750°C to 800°C, and the MT-TiCN layer is formed at 5 kPa to 15 kPa for 300 min to 400 min.
[0040] S3. Formation of intermediate TiCN layer: based on the total volume fraction of 100 vol%, the third reaction gas is a mixture of 10 vol% to 20 vol% TiCl4, 5 vol% to 10 vol% CH4 gas, 5 vol% to 10 vol% N2 gas, 0.5 vol% to 1 vol% CO gas, 0.5 vol% to 1 vol% AlCl3 gas and the remainder H2 gas. The mixed gas is adjusted and introduced into the reactor chamber. In the atmosphere of the third reaction gas, the temperature is set to 900°C to 1000°C, and the intermediate TiCN layer is formed for 20 min to 30 min at 5 kPa to 10 kPa. An intermediate layer with a concave and convex surface is formed on the surface of the titanium carbonitride layer (TiCN).
[0041] S4. Film formation of the Al2O3 layer: First, the nuclei of aluminum oxide crystals are formed. Based on the total volume fraction of 100 vol%, a mixture of 5 vol% to 15 vol% AlCl3 gas, 0.1 vol% to 1.2 vol% HCl gas, 0.1 vol% to 1.5 vol% CO2 gas and the remainder H2 gas is used. In this gas atmosphere, the temperature is set to 950°C to 1050°C, and nucleation is carried out at 5 kPa to 10 kPa for 3 min to 12 min.
[0042] Then, based on the total volume fraction of 100 vol%, the fourth reaction gas is a mixture of 5 vol% to 10 vol% AlCl3 gas, 0.5 vol% to 1.5 vol% HCl gas, 4 vol% to 5 vol% CO2 gas, 1 vol% H2S gas and the remainder H2 gas, and the mixed gas is adjusted and introduced into the reactor chamber, and the temperature is set to 950° C. to 1100° C. under the atmosphere of the fourth reaction gas, and the Al2O3 film is formed at 5 kPa to 10 kPa for 400 min to 500 min;
[0043] S5. Forming a TiN layer: Based on a total volume fraction of 100 vol%, the fifth reaction gas is a mixture of 2 vol% to 4 vol% TiCl4 gas, 25 vol% to 40 vol% N2 gas and the remainder H2 gas. The mixed gas is adjusted and introduced into the reactor chamber. In the atmosphere of the fifth reaction gas, the temperature is set to 960°C to 1100°C, and the film is formed at 30 kPa to 45 kPa for 60 min to 90 min.
[0044] After the coating is applied, the N2 gas is evacuated and the Ar gas is injected. The temperature is set to 1100℃~1300℃ and the pressure is 8MPa~10MPa for heat treatment. The treatment time is 2h~3h. After the heat treatment is completed, the power is turned off and the furnace is cooled to room temperature. The surface of the heat-treated coating is brushed on the cutting edge. Through this processing, the cutting edge is processed smoothly, the built-up edge is reduced, and the cutting resistance is reduced. The residual stress of the front blade coating is adjusted to 100MPa~-300MPa, and the residual stress of the back blade coating is adjusted to 50MPa~-500MPa. This ensures good wear resistance of the front blade and reduces the chipping caused by crescent wear. In addition, the overall coating greatly reduces the residual stress, so that the tool has a lower tensile stress or a certain compressive stress, which greatly improves the tool's anti-breakage performance.
[0045] Example 2: The cemented carbide coated tool of this example is prepared using the method of anti-breakage performance. First, prepare the cemented carbide substrate layer. Its preparation method is roughly the same as the general cemented carbide preparation. The cemented carbide coated tool material in this example is formulated with 80% WC powder, 10% metal Co powder and 10% compound powder of other metal components by weight. The compound powder of its metal component is at least one compound powder of Ti, Zr, Hf, Cr, Mo, Nb, Ta, Y and Si metal components. In this example, it is Mo and Cr elements, and the addition ratio is 1:1.
[0046] The preparation method is the same as that in Example 1, and the relative density of the blank substrate is strictly controlled to be 95.5% to 99.5%. The carbide blank blade is end-face ground, the edge is passivated, the end face is brushed, and finally cleaned to prepare for coating treatment.
[0047] The prepared carbide blank blade is then subjected to chemical vapor deposition (CVD) to form a film coating on the surface of the substrate. The total thickness of the composite coating is 10µm to 50µm, and the thickness of a single layer is 2µm to 10µm; the thickness of a single layer in this embodiment is 10µm.
[0048] The specific steps include: S1. forming a bottom TiN layer: based on a total volume fraction of 100 vol%, the first reaction gas is a mixture of 6 vol% to 8 vol% TiCl4 gas, 50 vol% to 60 vol% N2 gas and the remainder H2 gas, the mixed gas is adjusted and introduced into the reactor chamber, the temperature is set to 750° C. to 850° C., and the bottom TiN layer is formed in the atmosphere of the first reaction gas at 40 kPa to 50 kPa for 70 min to 80 min;
[0049] S2. MT-TiCN layer formation: based on a total volume fraction of 100 vol%, the second reaction gas is a mixture of 6 vol% to 10 vol% TiCl4 gas, 45 vol% to 55 vol% N2 gas, 2 vol% to 3 vol% CH3CN gas and the remainder H2 gas. The mixed gas is adjusted and introduced into the reactor chamber. Under the atmosphere of the second reaction gas, the temperature is set to 800° C. to 850° C., and the MT-TiCN layer is formed at 5 kPa to 10 kPa for 700 min to 900 min.
[0050] S3. Formation of intermediate TiCN layer: based on the total volume fraction of 100 vol%, the third reaction gas is a mixture of 25 vol% to 30 vol% TiCl4, 15 vol% to 20 vol% CH4 gas, 10 vol% to 15 vol% N2 gas, 0.5 vol% to 1 vol% CO gas, 2 vol% to 3 vol% AlCl3 gas and the remainder H2 gas. The mixed gas is adjusted and introduced into the reactor chamber. In the atmosphere of the third reaction gas, the temperature is set to 1000°C to 1050°C, and the intermediate TiCN layer is formed for 5 min to 15 min at 25 kPa to 40 kPa. An intermediate layer with a concave and convex surface is formed on the surface of the titanium carbonitride layer (TiCN).
[0051] S4. Film formation of the Al2O3 layer: First, to form the nucleus of the aluminum oxide crystal, based on the total volume fraction of 100 vol%, a mixture of 5 vol% to 15 vol% AlCl3 gas, 0.1 vol% to 1.2 vol% HCl gas, 4.5 vol% to 5.5 vol% CO2 gas and the remainder H2 gas is used. In this gas atmosphere, the temperature is set to 950°C to 1050°C, and nucleation is carried out at 5 kPa to 10 kPa for 3 min to 12 min.
[0052] Then, based on a total volume fraction of 100 vol%, the fourth reaction gas is a mixture of 10 vol% to 15 vol% AlCl3 gas, 3 vol% to 5 vol% HCl gas, 0.5 vol% to 1.5 vol% CO2 gas and the remainder H2 gas, and the mixed gas is adjusted and introduced into the reactor chamber, and in the atmosphere of the fourth reaction gas, the temperature is set to 950° C. to 1100° C., and the Al2O3 film is formed at 15 kPa to 20 kPa for 650 min to 800 min;
[0053] S5. Forming a TiN layer: Based on a total volume fraction of 100 vol%, the fifth reaction gas is a mixture of 8 vol% to 10 vol% TiCl4 gas, 45 vol% to 60 vol% N2 gas and the remainder H2 gas. The mixed gas is adjusted and introduced into the reactor chamber. In the atmosphere of the fifth reaction gas, the temperature is set to 960°C to 1100°C, and the film is formed at 70 kPa to 90 kPa for 30 min to 40 min.
[0054] After the coating is applied, it can be taken out of the furnace directly and put back into the pressure sintering furnace, where Ar gas is injected and the temperature is set to 1150℃~1200℃ and the pressure is 15MPa~20MPa for heat treatment. The treatment time is 4h~5h. After heat treatment, the defects of the substrate are removed and the tensile stress is relieved through reasonable design. The surface of the coating after heat treatment is brushed on the cutting edge. Through this processing, the cutting edge is smoothed, the built-up edge is reduced, and the cutting resistance is reduced. The residual stress of the front blade coating is adjusted to 100MPa~-300MPa, and the residual stress of the back blade coating is adjusted to 50MPa~-500MPa. The metallographic diagram of the cemented carbide tool material matrix is shown as follows. Figure 1 The metallographic diagram of the coating of cemented carbide tool material is shown in Figure 2As shown. The surface layer 1 can be coated with a colored layer (TiN layer) on the top surface for the convenience of color identification when using the tool; the aluminum oxide layer 2 is an anti-oxidation and wear-resistant layer, the transition layer 3 is the preparation of the aluminum oxide layer to improve adhesion, the TiCN layer 4 is a wear-resistant layer, and the TiN layer 5 is a primer to improve the adhesion of the coating. It is worth mentioning that the coating can be set in different combinations as needed, and can even be a single-layer structure.
[0055] Example 3: The cemented carbide coated tool of this example is prepared using the method of anti-breakage performance. First, prepare the cemented carbide substrate layer. Its preparation method is roughly the same as the general cemented carbide preparation. The cemented carbide coated tool material in this example is formulated with 90% WC powder, 5% metal Co powder and 5% compound powder of other metal components by weight. The compound powder of its metal component is at least one compound powder of Ti, Zr, Hf, Cr, Mo, Nb, Ta, Y and Si metal components. In this example, it is Nb and Ti elements, and the addition ratio is 1:1.
[0056] The preparation method is the same as that in Example 1, and the relative density of the blank substrate is strictly controlled to be 95.5% to 99.5%. The carbide blank blade is end-face ground, the edge is passivated, the end face is brushed, and finally cleaned to prepare for coating treatment.
[0057] The prepared cemented carbide blank blade is then subjected to chemical vapor deposition (CVD) to form a film coating on the surface of the substrate. The total thickness of the composite coating is 10µm to 50µm, and the thickness of a single layer is 2µm to 10µm; the thickness of a single layer in this embodiment is 8µm. The specific steps are the same as those in Example 2.
[0058] After coating, it can be taken out of the furnace directly and put back into the pressure sintering furnace, where Ar gas is injected and the temperature is set at 1250°C~1350°C and the pressure is 8MPa~10MPa for heat treatment for 2h~3h.
[0059] Comparative Example 1
[0060] Prepare the cemented carbide substrate layer. The raw material selection and preparation method are roughly the same as those of the cemented carbide preparation in Example 1. The difference from Example 1 is that the sintering process is fired at a temperature of 1380°C to 1520°C, the firing time is extended to 1h to 4h, and the relative density of the blank substrate is ensured to be 100%, thereby manufacturing a cemented carbide blank blade. The preparation method of the coating is the same as that of Example 1.
[0061] Comparative Example 2
[0062] Prepare a cemented carbide substrate layer. The raw material selection and preparation method are roughly the same as the cemented carbide preparation in Example 1. The relative density of the cemented carbide substrate layer is selected to be 95.5% to 99.5%, so that pores exist in the cemented carbide substrate layer. The preparation method for coating is the same as that in Example 1. The coating formula and process steps are the same as those in Example 1. The difference from Example 1 is that after the coating is applied, 40L / min of H2 is first passed through to cool for 2h, and then 40L / min of N2 is passed through to cool to room temperature and take out of the furnace. No heat treatment is used to eliminate pores after the coating is applied.
[0063] Comparative Example 3
[0064] The cemented carbide substrate layer is prepared. The raw material selection and preparation method are roughly the same as those of the cemented carbide preparation in Example 1. The difference from Example 1 is that the sintering process is sintered at a firing temperature of 1380°C to 1520°C, the firing time is extended to 1h to 4h, and the relative density of the blank matrix is ensured to be 100%, thereby manufacturing a cemented carbide blank blade.
[0065] The carbide blank blade is end-face ground, the edge is passivated, the end face is brushed, and finally cleaned in preparation for coating.
[0066] After the coating is applied, first pass H2 at 40 L / min to cool for 2 hours, then pass N2 at 40 L / min to cool to room temperature and then take out of the furnace.
[0067] The prepared cemented carbide coated cutting tools of Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3 were subjected to an intermittent cutting performance evaluation experiment.
[0068] Experimental verification:
[0069] Prepared tool model: WNMG080408-MT
[0070] Equipment used: Horizontal CNC lathe T5.2-500S
[0071] Experimental conditions:
[0072] Workpiece: material 42CrMo (Φ200×230mm, with 10mm wide groove×4 pieces);
[0073] Line speed (Vc): 150m / min;
[0074] Cutting depth (ap): 1.0mm;
[0075] Feed rate (f): 0.35 mm / r;
[0076] Others: wet (cutting fluid);
[0077] The number of impacts until the blade tip breaks (four impacts per feed) is shown in Table 1 below:
[0078]
[0079] It can be concluded from the test results in the above table that the impact resistance times of the cemented carbide coated tools in Examples 1 to 3 are significantly better than those of the cemented carbide coated tools in Comparative Examples 1 to 3. This shows that the method of the present invention can improve the anti-breakage performance of the entire product.
[0080] The above are only embodiments of the present invention. The invention is not limited to the field involved in this implementation case. The common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the content of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for improving the anti-breakage performance of cemented carbide coated cutting tools, characterized in that: According to the difference in expansion coefficients between the cemented carbide substrate layer and the coating material, the relative density of the cemented carbide substrate layer is adjusted to 95.5%~99.5%, so that pores exist in the cemented carbide substrate layer; the coated cemented carbide coated tool is heat treated to increase the shrinkage of the cemented carbide substrate layer; after the heat treatment, the cemented carbide substrate layer is cooled to eliminate the pores, reduce the tensile stress or change the compressive stress of the cemented carbide substrate layer, and alleviate the generation of cracks in the coating; the heat treatment process is to directly perform heat treatment after the coating is applied, at a temperature of 1100℃~1300℃, Ar gas pressure heat treatment, pressure of 8MPa~20MPa, and treatment time of 2h~5h; or after the coating is applied, it is taken out of the furnace and cooled to room temperature, and then put into the pressurized furnace again for heat treatment, the temperature is raised to 1150℃~1350℃, Ar gas pressure heat treatment, treatment pressure of 8MPa~20MPa, and treatment time of 2h~5h; The coating is a composite coating formed by alternately stacking TiN layers, TiCN layers and Al2O3 layers by chemical vapor deposition, and each layer of the composite coating is added with at least one trace element of Zr, Hf, Cr, Mo, Nb, Ta, Y, Si and W, and the value of the trace element in the molecular formula is between 0.05 and 0.
2.
2. The method for improving the anti-breakage performance of cemented carbide coated cutting tools according to claim 1, characterized in that: The total thickness of the composite coating is 10µm-50µm, and the thickness of a single layer is 2µm-30µm.
3. The method for improving the anti-breakage performance of cemented carbide coated cutting tools according to claim 2, characterized in that: The cemented carbide substrate layer includes refractory metal hard compound powder, bonding metal powder and compound powder of other metal components. By weight, the content of the refractory metal hard compound is 80% to 95%, the content of the bonding metal powder is 5% to 15%, and the content of the compound powder of other metal components is 0% to 15%.
4. The method for improving the anti-breakage performance of cemented carbide coated cutting tools according to claim 3, characterized in that: The refractory metal hard compound powder is WC powder, the bonding metal powder is at least one of Co powder and Ni powder, and the compound powder of other metal components is at least one of Ti, Zr, Hf, Cr, Mo, Nb, Ta, Y and Si metal components.
5. The method for improving the anti-breakage performance of cemented carbide coated cutting tools according to claim 4, characterized in that: The specific steps of the chemical vapor deposition method include: S1. Forming a bottom TiN layer: Based on a total volume fraction of 100 vol%, the first reaction gas is a mixture of 2 vol% to 8 vol% TiCl4 gas, 15 vol% to 65 vol% N2 gas and the remainder H2 gas, the temperature is set to 750°C to 950°C, and the bottom TiN layer is formed at 30 kPa to 50 kPa in the atmosphere of the first reaction gas for 40 min to 80 min; S2. MT-TiCN layer formation: based on a total volume fraction of 100 vol%, the second reaction gas is a mixture of 2 vol% to 10 vol% TiCl4 gas, 15 vol% to 65 vol% N2 gas, 1 vol% to 3 vol% CH3CN gas and the remainder H2 gas. Under the atmosphere of the second reaction gas, the temperature is set to 750°C to 850°C, and the MT-TiCN layer is formed at 5 kPa to 25 kPa for 300 min to 900 min. S3. Intermediate TiCN layer film formation: Based on the total volume fraction of 100 vol%, the third reaction gas is a mixture of 10 vol% to 30 vol% TiCl4, 5 vol% to 20 vol% CH4 gas, 5 vol% to 15 vol% N2 gas, 0.5 vol% to 1 vol% CO gas, 0.5 vol% to 3 vol% AlCl3 gas and the remainder H2 gas. In the atmosphere of the third reaction gas, the temperature is set to 900 ° C to 1050 ° C, and the intermediate TiCN layer is formed at 5 kPa to 40 kPa for 5 min to 30 min; S4. Forming an Al2O3 layer: First, forming a crystal nucleus of aluminum oxide crystals, and then, based on a total volume fraction of 100 vol%, a fourth reaction gas is composed of 5 vol% to 15 vol% AlCl3 gas, 0.5 vol% to 2.5 vol% HCl gas, 0.5 vol% to 5 vol% CO2 gas, 0 vol% to 1 vol% H2S gas and a remainder of H2 gas. In the atmosphere of the fourth reaction gas, the temperature is set to 950 ° C to 1100 ° C, and at 5 kPa to 20 kPa, the time is 400 min to 800 min to form an Al2O3 film; S5. Forming a TiN layer: Based on a total volume fraction of 100 vol%, the fifth reaction gas is a mixture of 2 vol% to 10 vol% TiCl4 gas, 25 vol% to 60 vol% N2 gas and the remainder H2 gas. Under the atmosphere of the fifth reaction gas, the temperature is set to 960°C to 1100°C, and the film is formed at 30 kPa to 85 kPa for 30 min to 90 min.
6. The method for improving the anti-breakage performance of cemented carbide coated cutting tools according to claim 5, characterized in that: The method for forming the nucleus of aluminum oxide crystals is: based on the total volume fraction of 100 vol%, a mixture of 5 vol% to 15 vol% AlCl3 gas, 0.1 vol% to 1.2 vol% HCl gas, 0.1 vol% to 5.5 vol% CO2 gas and the remainder H2 gas is used. Under this gas atmosphere, the temperature is set to 950°C to 1050°C, and nucleation is carried out at 5 kPa to 10 kPa for 3 min to 12 min.
7. A cemented carbide coated tool prepared by the method for improving the anti-breakage performance of cemented carbide coated tools according to any one of claims 1 to 6.