A self-supporting biomass carbon current collector, a composite current collector and its application

By using self-supporting biomass carbon current collectors in metallic lithium/sodium batteries and loading transition metal sulfides or selenides for modification, a three-dimensional porous structure is formed, which solves the problems of dendrite growth and volume expansion in lithium/sodium batteries and improves cycle performance. stability and energy density, achieving environmentally friendly and efficient battery performance improvements.

CN116014146BActive Publication Date: 2024-10-29HUAZHONG AGRI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211656780.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-29
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Existing metal lithium/sodium batteries have problems such as uneven deposition of lithium/sodium leading to dendrite growth, safety issues, unstable solid electrolyte interface and volume expansion, resulting in insufficient cycle life and energy density.

Method used

A self-supporting biomass carbon current collector is used and modified by loading transition metal sulfide or selenide to form a three-dimensional porous structure to uniformly guide lithium/sodium deposition, inhibit dendrite growth and alleviate volume expansion, and improve cycle stability.

Benefits of technology

The cycle life and rate performance of metallic lithium/sodium batteries are improved, the local current density is reduced, the growth of lithium/sodium dendrites is inhibited, the energy density and stability of the battery are improved, and biomass materials are environmentally friendly and widely sourced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116014146B_ABST
    Figure CN116014146B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of electrochemical energy, and specifically relates to a self-supporting biomass carbon current collector, a composite current collector and applications thereof. The self-supporting biomass carbon current collector is obtained by carbonizing a biomass material as a substrate under the protection of an inert gas. The self-supporting biomass carbon current collector has a high specific surface area and a natural vertical pore structure. After being modified by further loading lithium / sodium-philic transition metal sulfur / selenide and applied to the negative electrode of a metal lithium battery or a metal sodium battery, the local current density can be uniformed, and the uniform nucleation of lithium / sodium metal can be guided, thereby improving the cycle life and cycle rate performance of the metal lithium / sodium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrochemical energy, and in particular relates to a self-supporting biomass carbon current collector, a composite current collector and applications. Background Art

[0002] With the rapid development of fast-charging electronic devices and electric vehicles, people have put forward higher requirements for energy storage systems with higher capacity and higher energy density. However, the current commercial lithium-ion batteries based on intercalation reactions are difficult to meet people's growing demand for high energy density. Therefore, it is urgent to develop new secondary battery systems with high energy density and long cycle life. Compared with commercial lithium-ion battery anode graphite, the metallic lithium anode has an extremely high theoretical specific capacity (3860mAh / g), the lowest electrochemical potential (-3.04V, relative to the standard hydrogen electrode) and a smaller density (0.534g / cm 3 ) and has attracted widespread attention. Sodium, a member of the same main group, has similar physical and chemical properties to lithium and has also attracted research interest. However, there are many problems with metallic lithium / sodium anodes in practical applications: (1) The uneven deposition of lithium / sodium leads to the growth of lithium / sodium dendrites, which pierce the separator and cause the battery to short-circuit, causing safety issues; (2) The unstable solid electrolyte interface leads to the continuous consumption of metallic lithium / sodium and electrolyte, resulting in reduced coulombic efficiency; (3) Unlimited volume expansion leads to rapid capacity decay. Summary of the invention

[0003] In view of the above deficiencies in the prior art, the present invention provides a self-supporting biomass carbon current collector, a composite current collector and applications. The self-supporting biomass carbon current collector has a high specific surface area and a natural vertical pore structure. After being further loaded with transition metal sulfides and transition metal selenides for modification, it is applied to the negative electrode of a metal lithium battery or a metal sodium battery. It can uniformly distribute the local current density and guide the uniform nucleation of lithium / sodium metal, thereby improving the cycle life and cycle rate performance of the metal lithium / sodium battery.

[0004] Through research, the applicant found that constructing a three-dimensional current collector and modifying the surface of the current collector is an effective method to improve the performance of negative electrode materials for metal lithium / sodium batteries. On the one hand, the high specific surface area of ​​the three-dimensional current collector can reduce the local current density, evenly distribute the electric field, and inhibit the growth of lithium / sodium dendrites; on the other hand, the porous structure of the three-dimensional current collector can be used as a storage space for lithium / sodium, effectively alleviating the volume expansion of lithium / sodium metal during the cycle, thereby improving the cycle stability of metal lithium / sodium batteries. Carbon materials with high electronic conductivity and low mass density are ideal skeletons for accommodating metal lithium / sodium. Biomass carbon materials have the characteristics of wide sources, rich varieties, and environmental friendliness. Among them, woody plants of the arbor type have the characteristics of three-dimensional porosity and rich vertical channels, which can effectively inhibit the volume expansion of metal lithium / sodium negative electrodes, induce metal lithium / sodium to deposit inside, ensure that lithium / sodium ions are quickly and evenly deposited and stripped, and inhibit the growth of lithium / sodium dendrites.

[0005] Based on this, the present invention specifically provides a self-supporting biomass carbon current collector, which is obtained by taking biomass material as a substrate and undergoing carbonization treatment under the protection of an inert gas.

[0006] As a preferred embodiment, the biomass material is a woody plant of the tree type, such as at least one of Tilia, Metasequoia, Pinus tabulaeformis, Platycladus orientalis, and Populus, preferably Tilia.

[0007] As a preferred embodiment, the inert gas is nitrogen, argon or a hydrogen-argon mixture, preferably argon, the carbonization temperature is 500-1800°C, preferably 1300°C, the heating rate is 1-10°C / min, preferably 5°C / min, and the carbonization time is 0.5-10h, preferably 6h.

[0008] As a preferred embodiment, the thickness of the self-supporting biomass carbon current collector is 100-800 μm, preferably 400 μm.

[0009] As a preferred embodiment, the biomass material needs to be cultured with fungi, and the fungi are Pleurotus ostreatus hyphae, Aspergillus niger or yeast, preferably Pleurotus ostreatus hyphae.

[0010] As a preferred embodiment, the biomass material after fungal culture treatment needs to undergo pre-carbonization treatment under the protection of an inert gas; wherein the inert gas is nitrogen, argon or a hydrogen-argon mixture, preferably argon, the pre-carbonization temperature is 100-400°C, preferably 300°C, the heating rate is 1-10°C / min, preferably 5°C / min, and the pre-carbonization time is 0.5-5h, preferably 3h.

[0011] However, due to the lithium / sodium phobia of biomass carbon materials and the uneven distribution of lithium / sodium-philic sites, metallic lithium / sodium inevitably deposits preferentially on the surface of the three-dimensional current collector rather than inside, and the structural advantages of the three-dimensional current collector cannot be used to achieve uniform deposition of metallic lithium / sodium downward, and the induction effect on metallic lithium / sodium is lost during high capacity and long cycles. Therefore, it is necessary to modify the biocarbon material, and modify it with lithium / sodium-philic transition metal sulfur / selenide to provide uniform nucleation sites for the biomass carbon current collector, reduce the nucleation barrier, and induce uniform deposition of metallic lithium / sodium.

[0012] Based on this, the present invention also provides a composite current collector, which uses a self-supporting biomass carbon current collector as a precursor, and sequentially modifies transition metal sulfide nanoparticles or transition metal selenide nanoparticles on its surface through a solution immersion method and a high-temperature annealing method.

[0013] As a preferred embodiment, the transition metal sulfide nanoparticles or transition metal selenide nanoparticles are at least one of cobalt disulfide, iron disulfide, zinc sulfide, cobalt selenide, zinc selenide, and tin selenide, preferably cobalt selenide. When cobalt selenide is used, the content of cobalt selenide is 0.1-25% of the mass of the composite current collector, preferably 5%, and the particle size of the cobalt selenide is 50-500nm, preferably 200nm.

[0014] As a preferred embodiment, the solution immersion method comprises the following steps: immersing the self-supporting biomass carbon current collector in a mixed solution of a metal organic framework and a solvent; wherein the metal organic framework is at least one of ZIF-67, ZIF-5, and ZIF-8, preferably ZIF-67. The ZIF-67 comprises a cobalt source and an organic ligand 2-methylimidazole, wherein the cobalt source is Co(NO) 3 6H 2 O、CoCl 2 6H 2 O、(CH 3 COO 2 Co·4H 2 O, preferably Co(NO) 3 6H 2 O. The solvent is at least one of methanol, ethanol, acetone, propanol and water, preferably methanol. According to an embodiment of the present invention, the solution immersion time is 20-28h, preferably 2h.

[0015] As a preferred embodiment, the high-temperature annealing method includes the following steps: calcining the soaked self-supporting biomass carbon current collector and a selenium source or a sulfur source under the protection of an inert gas; wherein the selenium source is at least one of selenium powder, selenium chloride, and selenium sulfide, preferably selenium powder; the sulfur source is sulfur powder or thiourea, preferably sulfur powder; the inert gas is nitrogen, argon, or a hydrogen-argon mixture, preferably argon; the calcination annealing temperature is 500-1200°C, preferably 700°C, the heating rate is 1-10°C / min, preferably 5°C / min, and the calcination time is 1-5h, preferably 5h.

[0016] In addition, before the solution immersion method, the self-supporting biomass carbon current collector needs to be immersed in a strong acid solution to remove impurities, wash to neutrality, and dry. The strong acid solution is concentrated hydrochloric acid, concentrated sulfuric acid, concentrated nitric acid, preferably a concentrated hydrochloric acid solution, the concentration of the concentrated hydrochloric acid solution is 1-30wt%, preferably 10wt%, and the immersion time is 10-24h, preferably 12h. The impurity dissolution can be selected from the dispersion methods known in the art, such as stirring and dissolving. Preferably, the dissolution temperature is at room temperature. The dissolution time is 0.5-5h, for example, stirring at 25°C for 1h. The drying can be selected from the drying methods known in the art, such as blast drying or vacuum drying. Preferably, the drying temperature is 40-90°C, and the drying time is 12-24h, for example, blast drying at 80°C for 24h.

[0017] The present invention also provides an application of a composite current collector as a negative electrode of a metal lithium battery or a metal sodium battery, and lithium / sodium metal is deposited on the surface of the composite current collector at different current densities.

[0018] As a preferred embodiment, the current density is 0.1-20 mA / cm 2 , preferably 1-5 mA / cm 2 .

[0019] As a preferred solution, the deposition amount of the lithium / sodium metal is 0.1-30 mAh / cm 2 , preferably 10 mAh / cm 2 .

[0020] According to an embodiment of the present invention, a metal lithium battery or a metal sodium battery is prepared, which also needs to include a separator, a positive electrode plate and an electrolyte.

[0021] The electrolyte is selected from 1M LiTFSI+DOL / DME=1:1 (V:V)+1% LiNO 3 , 1M NaPF 6 +DEGDME, 1MLiPF 6 +EC / EMC / FEC=1:4:2(V:V:V).

[0022] The separator is at least one of a polypropylene separator, a glass fiber separator, a cellulose separator, and a polyethylene separator, and is preferably a polypropylene separator or a glass fiber separator.

[0023] The positive electrode sheet is coated on the current collector by the positive electrode material. The active material of the positive electrode material is at least one of lithium iron phosphate, lithium cobaltate, lithium manganate, lithium nickelate, NCM ternary material, and sodium vanadium phosphate, preferably lithium iron phosphate, NCM ternary material, and sodium vanadium phosphate. The positive electrode material also includes a conductive agent and a binder. Preferably, the conductive agent is selected from at least one of Super-P, acetylene black, and Ketjen black, preferably acetylene black. Preferably, the binder is selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR), preferably polyvinylidene fluoride. According to an embodiment of the present invention, the mass ratio of the active material, the conductive agent, and the binder is (7.5-8.5): (0.5-1.5): (0.5-1.5), preferably 80:10:10. According to an embodiment of the present invention, the current collector of the positive electrode sheet can be selected from a current collector known in the art, such as aluminum foil. The present invention also provides a method for preparing the positive electrode sheet, the preparation method comprising: coating the positive electrode material on a current collector, vacuum drying, and obtaining the positive electrode sheet. According to an embodiment of the present invention, the drying conditions are: a temperature of 50-90°C, and a drying time of 12-36h. Preferably, the drying conditions are: drying at 60°C for 24h.

[0024] According to an embodiment of the present invention, the operating temperature of the metal lithium / sodium battery is -20°C to 80°C, preferably 25°C.

[0025] The present invention has the following advantages: using a woody plant of the arbor type treated with fungi as a substrate, and obtaining a self-supporting biomass carbon current collector after high-temperature carbonization. By further loading a lithium / sodium-philic transition metal sulfur / selenide modification, the self-supporting biomass carbon current collector with a high specific surface area can effectively reduce the local current density during lithium / sodium deposition, inhibit the growth of lithium / sodium dendrites, and alleviate the volume expansion of the lithium / sodium negative electrode during the cycle. The low tortuosity and vertical pore structure of the self-supporting biomass carbon current collector can accommodate more lithium / sodium, thereby improving the surface capacity of the biomass carbon current collector. In addition, after the transition metal sulfur / selenide is in-situ grown and modified inside the pores of the self-supporting biomass carbon current collector, the lithium / sodium-philicity of the self-supporting biomass carbon current collector substrate can be improved, providing uniform nucleation sites, inducing lithium / sodium metal to preferentially deposit inside the pores of the self-supporting biomass carbon current collector substrate rather than on the surface, achieving uniform deposition of lithium / sodium metal, thereby improving the cycle stability of the metal lithium / sodium negative electrode. At the same time, the biomass precursors used are widely available, environmentally friendly, and have simple preparation methods; the modification methods used have simple process operations, low equipment requirements, and have good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The XRD spectra of the samples of Example 1 and Comparative Example 1 are shown in FIG.

[0027] Figure 2 This is a scanning electron microscope image of the sample in Example 1.

[0028] Figure 3 This is a scanning electron microscope image of the sample in Comparative Example 1.

[0029] Figure 4 For Example 1 and Comparative Example 1, 2 mA / cm 2 The current density is 10 mAh / cm 2 Coulombic efficiency cycle curve of lithium.

[0030] Figure 5 Deposition cells 10 mAh / cm for Example 1 and Comparative Example 1 2 The cycling performance diagram of the full battery assembled with lithium iron phosphate at 0.5C rate.

[0031] Figure 6 Deposition cells 10 mAh / cm for Example 1 and Comparative Example 1 2 Lithium and Li[Ni 0.8 Co 0.1 Mn 0.1 ]O 2 Cycling performance diagram of the assembled full battery. DETAILED DESCRIPTION

[0032] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0033] Embodiment 1:

[0034] The biomass carbon substrate described in this embodiment is linden, and the selected linden is only one of the woody plants of the tree class. If there are requirements for the structure and elemental composition of the biomass itself, then the corresponding woody plant of the tree class with a vertical pore structure can be selected. The transition metal sulfide and transition metal selenide described in the present invention are only one of the modified substances, which can be modified according to the characteristics of inducing lithium / sodium metal deposition. The method of this embodiment can also be applied to other woody plants with three-dimensional vertical pore structures and woody plants treated with fungi, and the application field of its products can also be expanded to the development of other types of secondary battery devices and non-energy storage fields that require carbon materials.

[0035] The trunk of the basswood tree was cut into thin slices and placed in a fungal culture medium. After 40 days, it was taken out, washed with ultrapure water to remove excess impurities on the surface, and dried in an 80°C blast oven. The dried basswood was placed in an argon atmosphere, heated to 300°C at a heating rate of 5°C / min, kept warm for 3 hours, and then heated to 1300°C at a heating rate of 5°C / min, and kept warm for 6 hours to obtain basswood slag carbon. After the material was cooled to room temperature, it was transferred to a beaker, washed with a 10wt% hydrochloric acid solution to remove impurities, then washed with distilled water until neutral, and dried. Use 800-mesh sandpaper to grind the basswood slag carbon to a thickness of 400μm. Weigh 383mg of 2-methylimidazole and dissolve it in 10mL of methanol, add the basswood slag carbon, stir for 30 minutes, and add 304mg Co(NO) 3 6H 2 O was dissolved in a solution of 10 mL of methanol and aged at room temperature for 24 hours. The basswood residue carbon soaked in the solution was placed in a tubular furnace in an Ar atmosphere, and selenium powder was added in a mass ratio of 1:1 to basswood residue carbon. The temperature was raised to 700°C at a heating rate of 5°C / min, and the mixture was kept for annealing for 2 hours. After cooling, the basswood residue carbon loaded with cobalt selenide was obtained. The morphological characteristics are shown in the attached Figure 2 Cut it into 0.8cm*0.8cm self-supporting electrode sheets, use lithium sheets as counter electrodes, assemble button batteries, and charge at 1mA / cm 2 The current density of deposition and stripping is 10 mAh / cm 2 The coulombic efficiency of the battery is tested. Figure 4 .

[0036] Lithium iron phosphate, acetylene black and polyvinylidene fluoride were weighed in a mass ratio of 8:1:1, and an appropriate amount of N-methylpyrrolidone was added and ground evenly in a mortar. The slurry was then coated on commercial aluminum foil with a scraper, placed in an oven at 60°C for vacuum drying, and sliced ​​into discs with a diameter of 10 mm. A matching deposition of 10 mA h / cm 2 After the lithium is loaded with cobalt selenide and the carbon negative electrode of basswood residue, it is assembled into a button metal lithium battery. The battery performance is shown in the attached Figure 5 .

[0037] Embodiment 2:

[0038] Weigh NCM ternary material, acetylene black and polyvinylidene fluoride in a mass ratio of 8:1:1, add an appropriate amount of N-methylpyrrolidone and grind evenly in a mortar. Then use a scraper to coat the slurry on commercial aluminum foil, place it in a 60°C oven for vacuum drying, and slice it into 10mm diameter discs. Matching deposition of 10mAh / cm 2 After the lithium is loaded with cobalt selenide and the basswood residue carbon negative electrode, it is assembled into a button metal lithium battery. The other steps are the same as in Example 1. The battery performance is shown in the attached Figure 6 .

[0039] Embodiment 3:

[0040] Cut the trunk of the basswood tree into thin slices, wash it with ultrapure water to remove excess impurities on the surface, and dry it in a blast oven at 80°C. Place the dried basswood in an argon atmosphere, heat it to 300°C at a heating rate of 5°C / min, keep it warm for 3 hours, and then heat it to 1300°C at a heating rate of 5°C / min, keep it warm for 6 hours, and obtain basswood slag carbon. After the material cools to room temperature, transfer it to a beaker, wash it with a 10wt% hydrochloric acid solution to remove impurities, then wash it with distilled water until it is neutral, and dry it. Use 800-mesh sandpaper to grind the basswood slag carbon to a thickness of 400μm. Weigh 383mg of 2-methylimidazole and dissolve it in 10mL of methanol, add the basswood slag carbon, stir for 30 minutes, and then add 304mg of Zn(NO) 3 6H 2 O was dissolved in a solution of 10 mL of methanol and aged at room temperature for 24 hours. The basswood residue carbon soaked in the solution was placed in a tubular furnace in an Ar atmosphere, and selenium powder was added in a mass ratio of 1:1 to basswood residue carbon. The temperature was raised to 700 °C at a heating rate of 5 °C / min, annealed for 2 hours, and cooled to obtain the basswood residue carbon material modified with zinc selenide.

[0041] The other steps are the same as in Example 1. Figure 4 .

[0042] Embodiment 4:

[0043] The basswood residue carbon loaded with cobalt selenide was cut into a 0.8 cm*0.8 cm self-supporting electrode sheet, and a button cell was assembled with a sodium sheet as the counter electrode. 2 The current density of deposition and stripping is 10 mAh / cm 2 The other steps are the same as in Example 1, and the coulombic efficiency is tested. The first cycle coulombic efficiency is 93.57%, and it can be stably circulated for 50 cycles.

[0044] Embodiment 5:

[0045] The basswood residue carbon loaded with cobalt selenide was cut into 0.8 cm*0.8 cm self-supporting electrode sheets, and a button cell was assembled with a lithium sheet as the counter electrode. 2 The current density of deposition and stripping is 20 mAh / cm 2 The other steps are the same as those in Example 1, and the coulombic efficiency is tested. The first cycle coulombic efficiency is 95.79%, and it can be stably cycled for 30 cycles.

[0046] Comparative Example 1:

[0047] The difference from Example 1 is that the basswood residue carbon is not modified with cobalt selenide. The other steps are the same as Example 1. The morphological characteristics are shown in the attached Figure 3 . At 1mA / cm 2 The current density of deposition and stripping is 10 mAh / cm 2 The coulombic efficiency of the battery is tested. Figure 4 . The deposited 10 mAh / cm 2 After the lithium-containing basswood residue carbon negative electrode is matched with the lithium iron phosphate positive electrode, a button metal lithium battery is assembled. The other steps are the same as in Example 1. The battery performance is shown in the attached Figure 5 .

[0048] Comparative Example 2:

[0049] The difference from Example 2 is that the basswood residue carbon is not modified with cobalt selenide, and the other steps are the same as Example 2. The battery performance is shown in the attached Figure 6 .

[0050] Comparative Example 3:

[0051] The difference from Example 1 is that the obtained basswood carbon material is loaded with cobalt selenide and has not been treated with fungi. Fungi secrete a variety of enzymes during reproduction, which selectively decompose lignin in the fiber tissue of the plant through the oxidation reaction of hydroxyl radicals, thereby increasing the proportion of its cellulose content. Compared with lignin, the cellulose carbon obtained by directly carbonizing cellulose has a higher degree of graphitization, and short-range ordered graphite-like carbon is obtained. However, basswood that has not been treated with fungi has a lower cellulose content and a higher lignin content, and the degree of graphitization of basswood carbon obtained after high-temperature carbonization is lower. At the same time, basswood carbon that has not been treated with fungi has a lower porosity and a lower differential pore volume, and cannot better uniformize the local current density and inhibit the growth of lithium dendrites. It was cut into a self-supporting electrode sheet of 0.8cm*0.8cm, and a lithium sheet was used as the counter electrode to assemble a button battery at 1mA / cm 2 The current density of deposition and stripping is 10 mAh / cm 2 The other steps are the same as in Example 1, and the coulombic efficiency is tested. The first cycle coulombic efficiency is 91.56%, and the cycle is stable for 50 cycles.

[0052] Comparative Example 4:

[0053] The difference from Example 1 is that the obtained basswood carbon material is neither loaded with cobalt selenide nor treated with fungi. It is cut into 0.8cm*0.8cm self-supporting electrode sheets, and a button cell is assembled with a lithium sheet as the counter electrode. 2 The current density of deposition and stripping is 10 mAh / cm 2 The other steps are the same as in Example 1, and the coulombic efficiency is tested. The first cycle coulombic efficiency is 91.60%, and it can be stably cycled for 30 cycles.

[0054] The present invention prepares a metal transition metal sulfur / selenide self-supporting carbon-based current collector with three-dimensional vertical channels, which can effectively solve the problems of dendrite growth and volume expansion of metal lithium / sodium negative electrodes during the cycle process. The metal transition metal sulfur / selenide acts as a nucleation site to induce the deposition of lithium / sodium inside the carbon channels of basswood residue instead of on the surface, promoting the uniform deposition of lithium / sodium.

[0055] Figure 1 The XRD spectra of Example 1 and Comparative Example 1 are shown in FIG. Figure 1 It can be seen that the three main diffraction peaks of Example 1 are at 33.2°, 44.8° and 50.4°, corresponding to the (101), (102) and (110) crystal planes of the CoSe standard card (PDF#70-2870), indicating the presence of CoSe in the carbon-based material. The XRD spectrum of Comparative Example 1 has two obvious broad peaks, corresponding to the (002) and (100) diffraction peaks of graphite, respectively. Figure 2 and Figure 3The scanning electron microscope photos of comparative example 1 and example 1 are respectively shown. Comparative example 1 has a low-tortuosity, vertically arranged pore structure, which is conducive to improving the wettability of the electrolyte, thereby accelerating the ion transfer rate and improving the coulombic efficiency of the battery. The cobalt selenide nanoparticles in example 1 are evenly distributed in the porous carbon layer, which can provide more lithium / sodium-philic sites to promote the uniform deposition of metallic lithium / sodium.

[0056] The half-cells of Example 1, Example 3 and Comparative Example 1 were assembled and the coulombic efficiency of metal lithium deposition was tested at a current density of 1 mA / cm 2 , the lithium deposition amount is 10mAh / cm 2 .from Figure 4 It can be seen that the composite current collector prepared by the present invention has higher first-cycle coulomb efficiency and cycle stability than the current collector of the comparative example, which indicates that the composite current collector provided by the present application improves the interface stability of lithium metal deposition and induces uniform deposition of metal lithium.

[0057] The deposition rate is 10 mAh / cm 2 The lithium metal Example 1 and Comparative Sample 1 were disassembled in a glove box, washed and dried, and then mixed with lithium iron phosphate, Li[Ni 0.8 Co 0.1 Mn 0.1 ]O 2 The positive electrode is matched to assemble the full battery. Figure 5 It can be seen that the lithium iron phosphate full battery assembled with the composite negative electrode of Example 1 has a higher capacity and a better capacity retention rate than that of Comparative Example 1. Figure 6 It can be seen that Example 1 has better rate performance.

Claims

1. A composite current collector, Features: Using a self-supporting biomass carbon current collector as a precursor, modifying the surface of the self-supporting biomass carbon current collector with transition metal sulfide nanoparticles or transition metal selenide nanoparticles by solution immersion method and high temperature annealing method in sequence; The self-supporting biomass carbon current collector is obtained by carbonizing a biomass material as a substrate under the protection of an inert gas; The biomass material is a woody plant of the tree type; The inert gas is nitrogen, argon or a mixture of hydrogen and argon, the carbonization temperature is 500-1800°C, the heating rate is 1-10°C / min, and the carbonization time is 0.5-10h; The thickness of the self-supporting biomass carbon current collector is 100-800 μm; The biomass material needs to be treated with fungus culture, and the fungus is oyster mushroom hyphae, black Aspergillus or yeast; The biomass material after fungal culture treatment needs to undergo pre-carbonization treatment under the protection of inert gas; wherein the inert gas is nitrogen, argon or a hydrogen-argon mixture, the pre-carbonization temperature is 100-400°C, the heating rate is 1-10°C / min, and the pre-carbonization time is 0.5-5h.

2. A composite current collector according to claim 1, Features: The transition metal sulfide nanoparticles or transition metal selenide nanoparticles are at least one of cobalt disulfide, iron disulfide, zinc sulfide, cobalt selenide, zinc selenide, and tin selenide.

3. A composite current collector according to claim 1, Features: The solution immersion method comprises the following steps: immersing the self-supporting biomass carbon current collector in a mixed solution of a metal organic framework and a solvent; wherein the metal organic framework is at least one of ZIF-67, ZIF-5, and ZIF-8; and the solvent is at least one of methanol, ethanol, acetone, propanol, and water; The high-temperature annealing method comprises the following steps: calcining the soaked self-supporting biomass carbon current collector and a selenium source or a sulfur source under the protection of an inert gas; wherein the selenium source is at least one of selenium powder, selenium chloride, and selenium sulfide; the sulfur source is sulfur powder or thiourea; the inert gas is nitrogen, argon, or a hydrogen-argon mixture; the calcination annealing temperature is 500-1200°C, the heating rate is 1-10°C / min, and the calcination time is 1-5h.

4. An application of the composite current collector according to claim 1, Features: As the negative electrode of metal lithium battery or metal sodium battery.

Citation Information

Patent Citations

  • Metal lithium composite material and preparing method thereof, and multilayer metal lithium composite material and preparing method thereof

    CN107732204A

  • Method for preparing carbon electrode material by constructing wood pore structure based on fungal method

    CN112927954A

  • Preparation method of Co0.85Se nanoparticle-coated 3D carbon network composite material and application of Co0.85Se nanoparticle-coated 3D carbon network composite material in lithium-sulfur battery

    CN114388814A