A multi-layered high brittle phase composite material and preparation method thereof

Through multi-layer structure design and multi-layer mixing hot pressing technology, the problem of easy fracture of highly brittle phase composite materials is solved, the tensile strength and toughness of the material are significantly improved, the mechanical properties are improved, and the preparation process is simplified.

CN116021859BActive Publication Date: 2024-10-18WUHAN UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310032626.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-10
Publication Date
2024-10-18
Estimated Expiration
2043-01-10

AI Technical Summary

Technical Problem

Existing highly brittle phase composite materials are prone to fracture due to excessive brittle phase content, especially when there are chips, scratches or internal defects, resulting in limited application of the material. The effect of solely relying on coupling agents to control the interface effect is limited and cannot be significantly improved. mechanical properties.

Method used

It adopts a multi-layer structure of highly brittle phase composite material design. The highly brittle material-resin composite layer and resin layer are alternately arranged, combined with multi-layer mixing hot pressing technology, to control the layered structure thickness and interface bonding to form a material with excellent mechanical properties. .

Benefits of technology

The tensile strength and toughness of the material are significantly improved. The dynamic tensile test results show that the tensile strength is increased by 206%. The process is simple and easy to implement, and has good designability and operability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004047509400000041
    Figure BDA0004047509400000041
  • Figure BDA0004047509400000051
    Figure BDA0004047509400000051
  • Figure HDA0004047509410000011
    Figure HDA0004047509410000011
Patent Text Reader

Abstract

The present invention relates to a multi-layer structured high-brittle phase composite material and a preparation method thereof. First, high-brittle materials such as barium sulfate and melamine are uniformly mixed with fluororesin and pressed into a series of single-layer sheets, and then the resin material is spread on one of the single-layer sheets and pre-pressed, and then another single-layer sheet is placed and pre-pressed in layers, and the resin is spread, the sheet is placed, and the pre-pressing operation is repeated several times, and finally a high-brittle phase composite material with a tensile strength of up to 4.6MPa at 20°C is obtained. The present invention adopts a multi-layer mixed material hot pressing technology to prepare composite materials with different macro structures. The entire preparation process is relatively simple, does not require the help of external field effects, is easy to implement and promote, and has strong designability and operability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of layered composite materials, and in particular to a multi-layered high-brittle phase composite material and a preparation method thereof. Background Art

[0002] With the increase of fuel economy and external load, the preparation of functionalized high-brittle matrix composites has gradually become a research hotspot for designers. High-brittle phase composites are brittle matrix composites composed of high-brittle phase matrix materials and a small amount of additives. They have the advantages of high strength, high modulus, excellent fracture toughness and stability. They are the development trend of the composite materials industry in recent years and are widely used in aerospace engine parts, polymer-based bonding explosive filling, transportation, building materials, buffer and shock-absorbing parts, etc.

[0003] Many high brittle phase composite materials are prone to fracture due to excessive content of specific brittle phases, especially in the presence of notches, scratches or internal defects, which greatly limits the widespread application of high brittle phase composite materials. In general, in order to obtain high brittle phase composite materials with excellent mechanical properties, a common method includes adding an adhesive to the matrix of the high brittle phase composite material and preparing a high brittle matrix composite material by bonding. The adhesive can improve the interface of the brittle phase matrix and effectively improve the bonding strength without affecting the equilibrium state of the material itself, thereby improving the mechanical strength of the material. In addition, hydrogen bonds and other effects can be generated between the high brittle phase matrix and the adhesive by coupling and other methods, which can serve as a "bridge" to improve the interface bonding. However, relying solely on the regulatory role of coupling agents and the like in the interface has limitations. This is because the bonding strength is not high and the distribution is uneven, the improvement effect is very limited, and it cannot play a substantial role in improvement. Summary of the invention

[0004] One of the purposes of the present invention is to provide a multi-layered high brittle phase composite material, which comprises at least two layers, which are composed of high brittle material-resin composite layers and resin layers arranged alternately in sequence.

[0005] Furthermore, the composite material has an even number of layers, preferably an even number between 2 and 16.

[0006] Furthermore, the resin raw materials used in each layer are the same or different, preferably the same.

[0007] Furthermore, the resin is selected from at least one of fluororesin, epoxy resin, phenolic resin and acrylic resin, preferably fluororesin, and more preferably a copolymer of vinylidene fluoride and chlorotrifluoroethylene in a mass ratio of 1:4.

[0008] Furthermore, the high brittle materials selected in the high brittle material-resin composite layer are the same or different, preferably the same.

[0009] Furthermore, the highly brittle material is selected from at least one of barium sulfate and melamine.

[0010] Furthermore, the high brittle material is specifically a mixture of barium sulfate and melamine, and the mass ratio of the two is 18-20:71-75, preferably 20:75.

[0011] Furthermore, the mass ratio of the high brittle material to the resin in the high brittle material-resin composite layer is 90-95:5-10, preferably 95:5, 94:6, 93:7, 92:8, 91:9, 90:10.

[0012] Furthermore, the ratio of the total mass of all resin layers to the mass of the entire composite material is 5-10:100.

[0013] Furthermore, the total thickness of the entire composite material and the thickness of a single resin layer are 29.40-30.50 mm and 0.04-1.11 mm, respectively.

[0014] The second object of the present invention is to provide a method for preparing the above-mentioned multi-layer structured high-brittle phase composite material, which mainly includes the following steps: (a) mixing the high-brittle material and the resin in a certain proportion and then flattening and pre-pressing them to obtain a single-layer pre-pressed thin sheet; (b) flattening the resin on the single-layer pre-pressed thin sheet and pre-pressing it, then placing another single-layer pre-pressed thin sheet, and then laminating and pre-pressing it; (c) repeating step (b), and finally hot pressing to form it.

[0015] Furthermore, in step (a), the average particle size of the highly brittle material is 20 μm-40 μm. The particle size of the highly brittle material must be within a suitable range. If it is too large, the density of the composite material will be too low.

[0016] Furthermore, in step (a), the pre-pressing temperature is room temperature, the pre-pressing pressure does not exceed 50 MPa, and the thickness of the sheet obtained by pre-pressing is 1.8 mm-15 mm.

[0017] Furthermore, in step (b), the lamination pre-pressing temperature is room temperature, and the lamination pre-pressing pressure does not exceed 50 MPa.

[0018] Furthermore, in step (c), the hot pressing molding temperature is 80-200° C. and the pressure is 1 GPa-4 GPa.

[0019] The present invention controls the thickness of the layered structure and performs hot pressing of the multilayered mixture at the glass transition temperature of the high brittle phase matrix, thereby finally obtaining a multilayer composite material with excellent mechanical properties. Through experimental comparison, it is found that during the stretching process, the interface bonding in the multilayer structure is tightly, uniformly and flat, and can maintain good bonding between layers. Compared with the single-layer structure composite material, the multilayer structure composite material greatly improves the strength of the material.

[0020] The beneficial effects of the present invention can be summarized as follows: (1) A multilayer mixing hot pressing technology is adopted to prepare composite materials with different macrostructures, and the multilayer structure can be flexibly designed and precisely controlled; (2) The dynamic tensile test results show that the multilayer high-brittle composite material prepared according to the method of the present invention has good tensile strength and toughness, and the tensile strength at 20°C can reach up to 4.6 MPa, which is 206% higher than that of a single-layer sample; (3) The integrated preparation process adopted by the present invention is relatively simple, does not require the help of an external field, is easy to implement and promote, and has strong designability and operability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The process flow chart and the real photos of the present invention are as follows;

[0022] Figure 2 is the stress-strain curve of the composite material sample obtained in Examples 1-5;

[0023] Figure 3 : are stress-strain curves of the composite material samples prepared in Examples 6-9;

[0024] Figure 4 10-13 are stress-strain curves of the composite material samples prepared in Examples 10-13;

[0025] Figure 5 The following are scanning electron microscope images of the composite material samples prepared in Examples 1-13. DETAILED DESCRIPTION

[0026] In order to enable ordinary technicians in the field to fully understand the technical solutions and beneficial effects of the present invention, further description is given below in conjunction with specific embodiments and drawings.

[0027] like Figure 1The preparation method of the multilayer structure high brittle phase composite material shown includes the following steps: the first step is to mix the high brittle material and the resin evenly, and then spread them flat in the mold, and use a hot press to pre-press them to obtain a single-layer pre-pressed sheet with a thickness of 1.80mm-15mm; the second step is to place a single-layer pre-pressed sheet in the mold, and then spread a layer of resin on its surface and pre-press it, and then put another single-layer pre-pressed sheet, and then use a hot press to stack and pre-press it; the third step is to repeat the second step several times according to the number of layers to be prepared, and finally hot press molding is performed under high temperature and high pressure.

[0028] The process conditions of Examples 1-13 are shown in Table 1 below.

[0029] Table 1 Comparison of process conditions of different embodiments

[0030]

[0031] The compositions of the multilayer structured high brittle phase composite materials obtained in Examples 1-13 are shown in Table 2 below.

[0032] Table 2 Comparison of the composition of the composite materials obtained in different embodiments

[0033]

[0034] In order to fully understand the performance of the layered high brittle phase composite materials obtained in each embodiment, the mechanical properties test and SEM electron microscope analysis were carried out on samples according to the method of GB / T 6329-1996 "Determination of tensile strength of adhesive butt joints". The results are as follows: Figure 2-5 shown.

[0035] from Figure 2-4 It can be seen from the stress-strain curve shown that as the number of layers increases, the tensile strength of the material increases, reaching a maximum at 8 layers, and when the interlayer resin content is 4%, the corresponding maximum tensile strength reaches 4.6 MPa (corresponding to Example 4).

[0036] Depend on Figure 5 It can be seen from the SEM photos that the present invention successfully constructs an interlayer resin structure, which deforms and absorbs energy during the stretching process, avoids stress concentration and improves the mechanical properties of the composite material.

Claims

1. A multilayer high brittle phase composite material, characterized in that: The composite material comprises at least two layers, which are formed by alternating arrangement of a high-brittle material-resin composite layer and a resin layer; the resin raw material selected in each layer is the same, and the resin is selected from at least one of fluororesin, epoxy resin, phenolic resin and acrylic resin; the high-brittle material selected in the high-brittle material-resin composite layer is a mixture of barium sulfate and melamine.

2. The composite material according to claim 1, characterized in that: The number of layers of the composite material is an even number between 2 and 16.

3. The composite material according to claim 1, characterized in that: The resin is specifically a copolymer of vinylidene fluoride and chlorotrifluoroethylene in a mass ratio of 1:4; the mass ratio of barium sulfate to melamine in the high-brittleness material is 18-20:71-75.

4. The composite material according to claim 1, characterized in that: The mass ratio of the high-brittle material to the resin in the high-brittle material-resin composite layer is 90-95:5-10.

5. The composite material according to claim 1, characterized in that: The ratio of the total mass of all resin layers to the mass of the entire composite material is 5-10:

100.

6. The composite material according to claim 1, characterized in that: The total thickness of the entire composite material and the thickness of a single resin layer are 29.40-30.50 mm and 0.04-1.11 mm, respectively.

7. A method for preparing a multilayer high brittle phase composite material according to any one of claims 1 to 6, characterized in that The method comprises the following steps: (a) mixing a highly brittle material and a resin in a uniform proportion, flattening and pre-pressing the mixture to obtain a single-layer pre-pressed sheet; (b) flattening and pre-pressing the resin on the single-layer pre-pressed sheet, placing another single-layer pre-pressed sheet, and then laminating and pre-pressing the sheet; (c) repeating step (b), and finally hot pressing to form the sheet.

8. The method according to claim 7, characterized in that: In step (a), the average particle size of the highly brittle material is 20 μm-40 μm, the pre-pressing temperature is room temperature, the pre-pressing pressure does not exceed 50 MPa, and the thickness of the pre-pressed sheet is 1.8 mm-15 mm.

9. The method according to claim 7, characterized in that: In step (b), the pre-pressing temperature of the laminate is room temperature, and the pre-pressing pressure of the laminate does not exceed 50 MPa; in step (c), the hot pressing molding temperature is 80-200° C., and the pressure is 1 GPa-4 GPa.

Citation Information

Patent Citations

  • Filler-reinforced solid resin multilayered structures

    CN109311293A