A carbon composite material and its preparation method and application, a lithium ion thermal battery

By using porous carbon and transition metal nitride quantum dot composite materials as cathode materials in lithium-ion thermal batteries, the problem of low thermoelectric conversion efficiency of existing cathode materials in lithium-ion thermal batteries is solved, and more efficient thermoelectric conversion and stability are achieved. .

CN116031383BActive Publication Date: 2024-10-29NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310028051.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-10-29
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

Existing lithium-ion thermal battery cathode materials have low thermoelectric conversion efficiency and complex integration processes, which limits the performance of thermoelectric conversion devices.

Method used

Porous carbon materials and transition metal nitride quantum dot composite materials are used as cathode materials for lithium-ion thermal batteries. Through the combination of hierarchical porous structure and transition metal nitride quantum dots, the conductivity and electrochemical effective specific surface area of ​​the material are improved, and thermoelectricity is enhanced. conversion efficiency.

Benefits of technology

It significantly improves the thermoelectric conversion efficiency and cycle stability of lithium-ion thermal batteries, increases the output voltage and thermal power, and improves the conductivity and electrochemical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116031383B_ABST
    Figure CN116031383B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium-ion batteries, and specifically relates to a carbon composite material, a preparation method and application thereof, and a lithium-ion thermal battery. The present invention provides a carbon composite material, comprising porous carbon and transition metal nitride quantum dots loaded on the porous carbon; the porous carbon has a multi-level pore structure. The porous carbon in the carbon composite material provided by the present invention has a multi-level pore structure, which can effectively shorten the transmission distance of electrolyte ions and electrons, facilitate the full infiltration of the electrolyte inside the electrode, and significantly increase the electrochemical effective specific surface area of ​​the electrode material; at the same time, the presence of transition metal nitride quantum dots improves the overall conductivity of the material; applying the carbon composite material provided by the present invention to a lithium-ion thermal battery can further improve the thermoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and specifically relates to a carbon composite material and a preparation method and application thereof, and a lithium ion thermal battery. Background Art

[0002] Thermal energy, as the most widely used energy in human production and life, is mostly dissipated in the form of low-quality heat (<100°C), which greatly reduces its utilization rate. Thermoelectric conversion devices can reuse this part of the dissipated low-quality heat and collect it in the form of electrical energy.

[0003] At present, commonly used thermoelectric conversion devices mainly use semiconductors as energy conversion carriers. Such devices are usually limited by their low thermoelectric conversion capacity, high hot end temperature and complex integration process.

[0004] Lithium-ion thermal batteries based on organic electrolyte systems are designed to have heat conductors on both sides of the positive and negative electrodes. During the charging process, the temperature of the heat conductors on both sides is changed to form a temperature gradient between the positive and negative electrodes, thereby forming an electromotive force between the positive and negative electrodes, prompting lithium ions to escape from the positive electrode and deposit at the negative electrode, completing the battery charging and achieving thermoelectric conversion.

[0005] However, the current positive electrode materials are mainly lithium iron phosphate, lithium titanate or lithium manganate, and the efficiency of thermoelectric conversion is low. Summary of the invention

[0006] The purpose of the present invention is to provide a carbon composite material and a preparation method and application thereof, and a lithium ion thermal battery. Applying the carbon composite material provided by the present invention to the thermal battery can further improve the thermoelectric conversion efficiency.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] The present invention provides a carbon composite material, comprising porous carbon and transition metal nitride quantum dots supported on the porous carbon;

[0009] The porous carbon has a multi-level pore structure.

[0010] Preferably, the transition metal element in the transition metal nitride includes one or more of molybdenum, vanadium, tungsten, chromium and niobium.

[0011] Preferably, the loading mass percentage of the transition metal nitride quantum dots is 5% to 15%.

[0012] Preferably, the multi-level pores include macroporous structure, mesoporous structure and microporous structure;

[0013] The volume ratio of the macroporous structure, the mesoporous structure and the microporous structure is 5-10:75-90:5-15.

[0014] The present invention also provides a method for preparing a carbon composite material, comprising the following steps:

[0015] A nitrogen source, a carbon source and a transition metal source are mixed and calcined to obtain the carbon composite material.

[0016] Preferably, the nitrogen source includes one or more of ammonium chloride, ammonium bicarbonate, ammonium carbonate, ammonium hydrogen phosphate and ammonium hydrogen sulfate;

[0017] The carbon source includes citrate;

[0018] The transition metal source includes a transition metal salt and / or a transition metal oxide;

[0019] The mass ratio of the nitrogen source, the carbon source and the transition metal source is 5:5:1-3.

[0020] Preferably, the calcination temperature is 700-1000°C and the holding time is 0.5-3h;

[0021] The calcination is carried out in a protective atmosphere.

[0022] The present invention also provides the use of the carbon composite material described in the above technical solution or the carbon composite material prepared by the preparation method described in the above technical solution in the positive electrode of a lithium-ion thermal battery.

[0023] The present invention also provides a lithium-ion thermal battery, comprising a battery unit and a heat conductor;

[0024] The battery unit includes a battery core and a battery shell wrapped around the outside of the battery core;

[0025] The battery core comprises a positive electrode, a separator and a negative electrode which are stacked in sequence; an electrolyte is filled between the positive electrode and the negative electrode;

[0026] The positive electrode comprises a current collector and a positive electrode material loaded on the current collector; the positive electrode material comprises an active material, a conductive agent and a binder; the active material is the carbon composite material described in the above technical solution or the carbon composite material prepared by the preparation method described in the above technical solution;

[0027] The heat conductor includes a first heat conductor and a second heat conductor; the first heat conductor and the second heat conductor are respectively arranged on both sides of the battery unit.

[0028] Preferably, the negative electrode comprises a lithium metal negative electrode;

[0029] The diaphragm includes a polypropylene diaphragm, a polyethylene diaphragm or a glass fiber diaphragm;

[0030] The heat conductor includes a Peltier.

[0031] The present invention provides a carbon composite material, comprising porous carbon and transition metal nitride quantum dots loaded on the porous carbon; the porous carbon has a multi-level pore structure. The porous carbon in the carbon composite material provided by the present invention has a multi-level pore structure, which can effectively shorten the transmission distance of electrolyte ions and electrons, facilitate the full infiltration of the electrolyte inside the electrode, and significantly increase the electrochemical effective specific surface area of ​​the electrode material; at the same time, the presence of the transition metal nitride quantum dots improves the overall conductivity of the material. Since the electrical conductivity of the material is positively correlated with the thermoelectric conversion efficiency, the carbon composite material provided by the present invention is applied to the positive electrode of a lithium-ion thermal battery, which can further improve the thermoelectric conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the structure of the lithium-ion thermal battery obtained in the application example, wherein 1-first Peltier, 2-aluminum-plastic film, 3-negative electrode, 4-diaphragm, 5-positive electrode, 6-second Peltier, 7-negative electrode tab, 8-positive electrode tab;

[0033] Figure 2 is a SEM image of the carbon composite material obtained in Example 1;

[0034] Figure 3 is the XRD pattern of the carbon composite material obtained in Example 1;

[0035] Figure 4 The voltage variation diagram of the lithium ion thermal battery assembled with the carbon composite material obtained in Example 1 and Comparative Examples 1-2 under different temperature differences;

[0036] Figure 5 The voltage variation diagram of the lithium-ion thermal battery assembled with the carbon composite material obtained in Examples 6 to 7 under different temperature differences;

[0037] Figure 6 This is a graph of the Seebeck coefficient of a lithium-ion thermal battery assembled from the carbon composite materials obtained in Example 1 and Comparative Examples 1-2 at different temperature differences;

[0038] Figure 7 This is a graph of the Seebeck coefficient of a lithium-ion thermal battery assembled from the carbon composite material obtained in Examples 6 to 7 at different temperature differences;

[0039] Figure 8 The test curve of thermal charge-load discharge of the lithium ion thermal battery assembled with the carbon composite material obtained in Example 1 and Comparative Examples 1-2;

[0040] Fig. 9The test curve of thermal charge-load discharge of the lithium-ion thermal battery assembled with the carbon composite material obtained in Examples 6 to 7;

[0041] Fig.10 This is a graph of the output thermal power of a lithium-ion thermal battery assembled from the carbon composite materials obtained in Example 1 and Comparative Examples 1-2;

[0042] Fig.11 This is the output thermal power diagram of the lithium-ion thermal battery assembled with the carbon composite material obtained in Examples 6 to 7;

[0043] Fig.12 is a thermogravimetric analysis curve of the carbon composite material obtained in Example 1;

[0044] Fig.13 The nitrogen adsorption-desorption curves of the carbon composite material obtained in Example 1 and the porous carbon material obtained in Comparative Examples 1-2;

[0045] Fig.14 These are pore size test curves of the carbon composite material obtained in Example 1 and the porous carbon material obtained in Comparative Examples 1-2. DETAILED DESCRIPTION

[0046] The present invention provides a carbon composite material, comprising porous carbon and transition metal nitride quantum dots supported on the porous carbon;

[0047] The porous carbon has a multi-level pore structure.

[0048] In the present invention, the multi-level pores preferably include a macroporous structure, a mesoporous structure and a microporous structure; the volume ratio of the macroporous structure, the mesoporous structure and the microporous structure is preferably 5-10:75-90:5-15.

[0049] In the present invention, the specific surface area of ​​the carbon composite material is preferably 300 to 2000 m 2 In the present invention, the particle size of the carbon composite material is preferably 5 to 10 μm.

[0050] In the present invention, the transition metal element in the transition metal nitride preferably includes one or more of molybdenum, vanadium, tungsten, chromium and niobium.

[0051] In the present invention, the transition metal nitride quantum dots preferably have a pure phase structure of a monoclinic system. In the present invention, the particle size of the transition metal nitride quantum dots is preferably 3 to 10 nm, more preferably 4 to 9 nm, and more preferably 5 to 8 nm.

[0052] In the present invention, the loading mass percentage of the transition metal nitride quantum dots is preferably 5% to 15%, more preferably 7% to 12%, and even more preferably 8% to 10%.

[0053] The present invention also provides a method for preparing the carbon composite material described in the above technical solution, comprising the following steps:

[0054] A nitrogen source, a carbon source and a transition metal source are mixed and calcined to obtain the carbon composite material.

[0055] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0056] In the present invention, the nitrogen source preferably includes one or more of ammonium chloride, ammonium bicarbonate, ammonium carbonate, ammonium hydrogen phosphate and ammonium hydrogen sulfate; when the nitrogen source is two or more of the above options, the present invention has no special limitation on the ratio of the specific substances, and they can be mixed in any ratio.

[0057] In the present invention, the carbon source preferably includes citrate. In the present invention, the citrate preferably includes one or more of sodium citrate and potassium citrate.

[0058] In the present invention, the transition metal source preferably includes a transition metal salt and / or a transition metal oxide. In the present invention, the transition metal salt preferably includes a transition metal sodium salt, a transition metal potassium salt or a transition metal ammonium salt. In the present invention, the transition metal salt preferably includes one or more of molybdate, tungstate, vanadate, chromate and niobate; the transition metal oxide preferably includes one or more of molybdenum trioxide, tungsten trioxide, vanadium pentoxide and niobium pentoxide.

[0059] In the present invention, the mass ratio of the nitrogen source, the carbon source and the transition metal source is preferably 5:5:1-3, and more preferably 5:5:2.

[0060] In the present invention, the mixing is preferably carried out at room temperature. In the present invention, the mixing method is preferably grinding; the grinding time is preferably 30 minutes. The present invention has no special limitation on the grinding process, and the grinding process can be carried out using a process well known to those skilled in the art. In the present invention, the grinding is preferably carried out in a mortar.

[0061] In the present invention, the calcination temperature is preferably 700-1000°C, more preferably 750-950°C, and more preferably 800-900°C; the heating rate to the calcination temperature is preferably 2°C / min; the holding time is preferably 0.5-3h, more preferably 1.0-2.5h, and more preferably 1.5-2.0h.

[0062] In the present invention, the calcination is preferably carried out in a protective atmosphere; the protective atmosphere preferably includes nitrogen.

[0063] After the calcination, the present invention also preferably includes washing, filtering and drying the obtained material. The present invention has no special limitation on the washing and filtering process, and the process well known to those skilled in the art can be used. In the present invention, the drying temperature is preferably 80°C, the time is preferably 12 hours; the drying is preferably vacuum drying.

[0064] The present invention also provides the use of the carbon composite material described in the above technical solution or the carbon composite material prepared by the preparation method described in the above technical solution in the positive electrode of a lithium-ion thermal battery.

[0065] The present invention also provides a lithium-ion thermal battery, comprising a battery unit and a heat conductor;

[0066] The battery unit includes a battery core and a battery shell wrapped around the outside of the battery core;

[0067] The battery core comprises a positive electrode, a separator and a negative electrode which are stacked in sequence; an electrolyte is filled between the positive electrode and the negative electrode;

[0068] The positive electrode comprises a current collector and a positive electrode material loaded on the current collector; the positive electrode material comprises an active material, a conductive agent and a binder; the active material is the carbon composite material described in the above technical solution or the carbon composite material prepared by the preparation method described in the above technical solution;

[0069] The heat conductor includes a first heat conductor and a second heat conductor; the first heat conductor and the second heat conductor are respectively arranged on both sides of the battery unit.

[0070] In the present invention, the conductive agent preferably includes acetylene black and / or Ketjen black; the binder preferably includes sodium carboxymethylcellulose and / or polyvinylidene fluoride. In the present invention, the mass ratio of the active material, the conductive agent and the binder is preferably 8:1:1.

[0071] In the present invention, the method for preparing the positive electrode preferably comprises the following steps:

[0072] The active material, the conductive agent, the binder and water are mixed, the obtained slurry is coated on the surface of the current collector, and the positive electrode is obtained after drying.

[0073] The present invention has no particular limitation on the concentration of the slurry and the coating method, and those known to those skilled in the art may be used. In the present invention, the drying temperature is preferably 60° C. and the drying time is preferably 12 hours.

[0074] In the present invention, the loading amount of the positive electrode material on the positive electrode is preferably 1.5 to 2 mg / cm 2 In the present invention, the positive electrode is preferably a disc with a diameter of 1.2 cm.

[0075] In the present invention, the negative electrode preferably includes a lithium metal negative electrode.

[0076] In the present invention, the positive electrode and the negative electrode are preferably independently provided with electrode tabs.

[0077] In the present invention, the diaphragm preferably includes a polypropylene diaphragm, a polyethylene diaphragm or a glass fiber film. In the present invention, the electrolyte preferably includes a LiPF6 electrolyte, a LiTFSI electrolyte or a LiFSI electrolyte; the concentration of the electrolyte is preferably 1 mol / L. In a specific embodiment of the present invention, the electrolyte is preferably a 1 mol / L LiPF6 electrolyte, and the solvent of the electrolyte is EC / DMC / EMC in a volume ratio of 1:1:1.

[0078] In the present invention, the battery shell is preferably an aluminum-plastic film. The present invention has no special limitation on the packaging method of the battery shell, and any method known to those skilled in the art can be used.

[0079] In the present invention, the heat conductor preferably includes a Peltier.

[0080] The present invention has no special limitation on the assembly method of the lithium-ion thermal battery, and the assembly can be directly performed in a glove box filled with nitrogen according to the structure of the battery.

[0081] The lithium ion thermal battery provided by the present invention does not need to provide an additional power supply when the battery is charged after discharge. By heating the heat conductor on the positive electrode side of the thermal battery and controlling the heat conductor on the negative electrode side at room temperature, a certain temperature gradient is formed between the positive and negative electrodes, and then an electromotive force is formed between the positive and negative electrodes, which promotes the lithium ions to escape from the positive electrode and deposit on the negative electrode, thereby realizing the charging of the battery.

[0082] In order to further illustrate the present invention, a carbon composite material, a preparation method and application thereof, and a lithium-ion thermal battery provided by the present invention are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0083] Example 1

[0084] 2.5 g of ammonium chloride, 2.5 g of sodium citrate and 1.0 g of sodium molybdate were placed in a mortar and ground for 30 min. The mixture was heated to 800 °C at a heating rate of 2 °C / min under a nitrogen atmosphere and calcined for 2 h. The calcined product was washed and filtered in turn and vacuum dried at 80 °C for 12 h to obtain a carbon composite material (the particle size of the Mo2N quantum dots is 4 nm, the loading percentage is 8.9%, and the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 5:80:15).

[0085] Example 2

[0086] 2.5 g of ammonium chloride, 2.5 g of potassium citrate and 1.0 g of sodium molybdate were placed in a mortar and ground for 30 min. The mixture was heated to 800 °C at a heating rate of 2 °C / min under a nitrogen atmosphere and calcined for 2 h. The calcined product was washed and filtered in turn and vacuum dried at 80 °C for 12 h to obtain a carbon composite material (the particle size of the Mo2N quantum dots is 4 nm, the loading percentage is 8%, and the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 8:81:11).

[0087] Example 3

[0088] 2.5 g of ammonium chloride, 2.5 g of potassium citrate and 1.0 g of sodium molybdate were placed in a mortar and ground for 30 min. The mixture was heated to 800 °C at a heating rate of 2 °C / min under a nitrogen atmosphere and calcined for 2 h. The calcined product was washed and filtered in turn and vacuum dried at 80 °C for 12 h to obtain a carbon composite material (the particle size of the Mo2N quantum dots is 4 nm, the loading percentage is 8%, and the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 10:84:6).

[0089] Example 4

[0090] 2.5 g of ammonium chloride, 2.5 g of sodium citrate and 1.0 g of potassium molybdate were placed in a mortar and ground for 30 min. The mixture was heated to 800 °C at a heating rate of 2 °C / min under a nitrogen atmosphere and calcined for 2 h. The calcined product was washed and filtered in turn and vacuum dried at 80 °C for 12 h to obtain a carbon composite material (the particle size of the Mo2N quantum dots is 4 nm, the loading percentage is 8.6%, and the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 8:81:11).

[0091] Example 5

[0092] 2.5 g of ammonium chloride, 2.5 g of sodium citrate and 1.0 g of ammonium molybdate were placed in a mortar and ground for 30 min. The mixture was heated to 800 °C at a heating rate of 2 °C / min under a nitrogen atmosphere and calcined for 2 h. The calcined product was washed and filtered in turn and vacuum dried at 80 °C for 12 h to obtain a carbon composite material (the particle size of the Mo2N quantum dots is 5 nm, the loading percentage is 7%, and the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 8:83:9).

[0093] Example 6

[0094] 2.5 g of ammonium chloride, 2.5 g of sodium citrate and 0.5 g of sodium molybdate were placed in a mortar and ground for 30 min. The mixture was heated to 800 ° C at a heating rate of 2 ° C / min under a nitrogen atmosphere and calcined for 2 h. The calcined product was washed and filtered in turn, and vacuum dried at 80 ° C for 12 h to obtain a carbon composite material (the particle size of Mo2N quantum dots is 4 nm, the loading percentage is 5%, and the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 3:90:7).

[0095] Example 7

[0096] 2.5 g of ammonium chloride, 2.5 g of sodium citrate and 1.5 g of sodium molybdate were placed in a mortar and ground for 30 min. The mixture was heated to 800 ° C at a heating rate of 2 ° C / min under a nitrogen atmosphere and calcined for 2 h. The calcined product was washed and filtered in turn, and vacuum dried at 80 ° C for 12 h to obtain a carbon composite material (the particle size of Mo2N quantum dots is 8 nm, the loading percentage is 15%, and the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 5:85:10).

[0097] Comparative Example 1

[0098] 2.5 g of ammonium chloride and 2.5 g of sodium citrate were placed in a mortar and ground for 30 minutes. The resulting mixture was heated to 800°C at a heating rate of 2°C / min under a nitrogen atmosphere and calcined for 2 hours. The calcined product was washed and filtered in turn, and vacuum dried at 80°C for 12 hours to obtain nitrogen-doped porous carbon (the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 2:88:10).

[0099] Comparative Example 2

[0100] 2.5 g of sodium citrate was placed in a mortar and ground for 30 minutes. The mixture was heated to 800°C in a nitrogen atmosphere at a heating rate of 2°C / min and calcined for 2 hours. The calcined product was washed and filtered in turn, and vacuum dried at 80°C for 12 hours to obtain porous carbon (the volume ratio of the macroporous structure, mesoporous structure and microporous structure in the porous carbon is 11:87:2).

[0101] Application Examples

[0102] The carbon composite material obtained in Examples 1, 6, 7 and Comparative Examples 1-2 was used as the active material. The active material, acetylene black and sodium carboxymethyl cellulose were mixed in a ratio of 8:1:1, and then water was added to grind them into a paste to obtain a slurry; the obtained slurry was coated on a copper foil, dried at 60°C for 12 hours, and then cut into discs with a diameter of 1.2 cm as the positive electrode (the loading amount of the positive electrode material was 2 mg / cm 2 );

[0103] A lithium metal sheet is used as the negative electrode, a polypropylene film is used as the separator, 1M LiPF6 (EC / DMC / EMC volume ratio is 1:1:1) is used as the electrolyte, and an aluminum plastic film is used as the battery shell. The battery is assembled in a glove box filled with nitrogen, and Peltiers are set on both sides of the battery to obtain a lithium-ion thermal battery. The structure of the lithium-ion thermal battery is as follows Figure 1 As shown, 1 is the first Peltier, 2 is the aluminum-plastic film, 3 is the negative electrode, 4 is the separator, 5 is the positive electrode, 6 is the second Peltier, 7 is the negative electrode tab, and 8 is the positive electrode tab.

[0104] Performance Testing

[0105] Test Example 1

[0106] The carbon composite material obtained in Example 1 was tested by scanning electron microscopy, and the obtained SEM image is as follows: Figure 2 As shown, from Figure 2 It can be seen that the carbon composite material provided by the present invention is a three-dimensional porous carbon composite structure rich in Mo2N quantum dots, with abundant pores and uniform pore size, wherein the size of Mo2N is about 4 nm.

[0107] Test Example 2

[0108] The carbon composite material obtained in Example 1 was subjected to an X-ray diffraction test, and the obtained XRD pattern is as follows: Figure 3 As shown, from Figure 3 It can be seen that a pure phase Mo2N having a monoclinic crystal structure is formed in the carbon composite material provided by the present invention.

[0109] Test Example 3

[0110] The voltage change of the lithium-ion thermal battery obtained in the test application example under different temperature differences is shown in the following figure. Figures 4-5 As shown;

[0111] Figure 4 The application example represents embodiment 1, from Figure 4 It can be seen that the output voltage of the thermal battery is positively correlated with the temperature difference, and when the temperature difference is 25K, an output voltage as high as 1.6V can be obtained, which is significantly higher than the results obtained in Comparative Examples 1 to 2;

[0112] from Figure 5It can be seen that the output voltage of Example 6 when the temperature difference is 25K is 1.3V, and the output voltage of Example 7 when the temperature difference is 25K is 1.4V;

[0113] It should be noted that before thermal charging, the entire device was first electrochemically discharged to 0.01 V at a current density of 0.1 A / g.

[0114] Test Example 4

[0115] The Seebeck coefficient of the lithium-ion thermal battery obtained in the application example under different temperature differences is calculated by the formula S = ΔV / ΔT. The obtained curve is as follows Figures 6-7 As shown;

[0116] Figure 6 The application example represents embodiment 1, from Figure 6 It can be seen that the Seebeck coefficient is as high as 57.3 mV / K, while the Seebeck coefficients of Comparative Example 1 and Comparative Example 2 are 39.7 mV / K and 7.2 mV / K respectively;

[0117] from Figure 7 It can be seen that the Seebeck coefficients of Examples 6 to 7 can reach 28.7 mV / K and 24.2 mV / K respectively;

[0118] The above results show that the thermoelectric conversion capacity of lithium-ion thermal batteries can be effectively improved by combining molybdenum nitride quantum dots with porous carbon.

[0119] Test Example 5

[0120] The lithium-ion thermal battery obtained in the corresponding case is subjected to a thermal charge-load discharge test, and the obtained curve is as follows Figures 8-9 As shown;

[0121] Figure 8 The application example in the embodiment 1 is representative, from Figure 8 It can be seen that the lithium-ion thermal battery obtained in Example 1 can maintain a voltage of 1.6 to 1.7 V after 50 cycles of thermal charging when the load is 10 kΩ; Fig. 9 It can be seen that the voltage of Example 6 can still be stably maintained at 1.2-1.25V after cycling, while the hot charging voltage of Example 7 increases significantly during the cycling process and eventually reaches 1.1V, which may be due to the gradual activation of the electrode material; it should be noted that the hot charging voltage of Comparative Examples 1 and 2 decays significantly after 50 cycles, and can only be maintained at 0.7V and 0.35V in the end;

[0122] The above results show that the lithium-ion thermal battery obtained by the present invention has good cycle stability and practicality.

[0123] Test Example 6

[0124] The output power of the lithium-ion thermal battery obtained in the corresponding case is tested, and the obtained curve is as follows Figures 10-11 As shown;

[0125] Fig.10 The application example in the embodiment 1 is representative, from Fig.10 It can be seen that compared with the thermoelectric conversion power (0.3 mW, 0.05 mW) of the lithium ion thermal battery obtained in Comparative Examples 1 to 2, the lithium ion thermal battery obtained in Example 1 of the present invention can obtain a maximum thermoelectric conversion power of 0.7 mW when the load is 10 kΩ;

[0126] from Fig.11 It can be seen that Examples 6 to 7 can output a maximum thermoelectric conversion power of 0.37 mW and 0.15 mW, respectively.

[0127] Test Example 7

[0128] The carbon composite material in Example 1 was subjected to a thermogravimetric analysis test in air atmosphere, and the test curve obtained was as follows: Fig.12 As shown, from Fig.12 It can be seen that the content of molybdenum nitride in the carbon composite is 8.9%.

[0129] Test Case 8

[0130] The specific surface areas of the carbon composite material obtained in Example 1 and the porous carbon material obtained in Comparative Examples 1 to 2 were tested by nitrogen adsorption / desorption method. The test curves obtained are as follows: Fig.13 As shown, from Fig.13 It can be seen that the specific surface area of ​​the carbon composite material obtained in Example 1 is 339 m 2 / g, the specific surface areas of the porous carbon materials obtained in Comparative Examples 1 and 2 were 321 m 2 / g and 128m 2 / g.

[0131] Test Example 9

[0132] The pore sizes of the carbon composite material obtained in Example 1 and the porous carbon materials obtained in Comparative Examples 1 to 2 were tested, and the test curves obtained were as follows: Fig.14 As shown, from Fig.14 It can be seen that the pore size of the carbon composite material obtained in Example 1 is mainly distributed in the range of micropores, mesopores and macropores, and has a graded porous characteristic.

[0133] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. Application of a carbon composite material in a positive electrode of a lithium-ion thermal battery, characterized in that: The lithium-ion thermal battery comprises a battery cell and a heat conductor; The battery unit includes a battery core and a battery shell wrapped around the outside of the battery core; The battery core comprises a positive electrode, a separator and a negative electrode which are stacked in sequence; an electrolyte is filled between the positive electrode and the negative electrode; The positive electrode comprises a current collector and a positive electrode material loaded on the current collector; the positive electrode material comprises an active material, a conductive agent and a binder; the active material is a carbon composite material; The heat conductor comprises a first heat conductor and a second heat conductor; the first heat conductor and the second heat conductor are respectively arranged on both sides of the battery unit; The carbon composite material comprises porous carbon and transition metal nitride quantum dots supported on the porous carbon; The porous carbon has a multi-level pore structure; The transition metal in the transition metal nitride is molybdenum; The method for preparing the carbon composite material comprises the following steps: Mixing a nitrogen source, a carbon source and a transition metal source, and calcining the mixture to obtain the carbon composite material; The mixing method is grinding; The nitrogen source includes one or more of ammonium chloride, ammonium bicarbonate, ammonium carbonate, ammonium hydrogen phosphate and ammonium hydrogen sulfate; The carbon source includes citrate; The transition metal source includes a transition metal salt and / or a transition metal oxide.

2. The use according to claim 1, characterized in that: The loading mass percentage of the transition metal nitride quantum dots is 5% to 15%.

3. The use according to claim 1, characterized in that: The multi-level pores include macroporous structure, mesoporous structure and microporous structure; The volume ratio of the macroporous structure, the mesoporous structure and the microporous structure is 5-15:75-90:5-10.

4. The use according to claim 1, characterized in that: The mass ratio of the nitrogen source, the carbon source and the transition metal source is 5:5:1-3.

5. The use according to claim 1, characterized in that: The calcination temperature is 700-1000°C, and the holding time is 0.5-3h; the calcination is carried out in a protective atmosphere.

6. A lithium-ion thermal battery, characterized in that: including a battery cell and a heat conductor; The battery unit includes a battery core and a battery shell wrapped around the outside of the battery core; The battery core comprises a positive electrode, a separator and a negative electrode which are stacked in sequence; an electrolyte is filled between the positive electrode and the negative electrode; The positive electrode comprises a current collector and a positive electrode material loaded on the current collector; the positive electrode material comprises an active material, a conductive agent and a binder; the active material is a carbon composite material according to any one of claims 1 to 5; The heat conductor includes a first heat conductor and a second heat conductor; the first heat conductor and the second heat conductor are respectively arranged on both sides of the battery unit.

7. The lithium-ion thermal battery according to claim 6, characterized in that: The negative electrode comprises a lithium metal negative electrode; The diaphragm includes a polypropylene diaphragm, a polyethylene diaphragm or a glass fiber diaphragm; The heat conductor includes a Peltier.