A method for preparing a high-performance photocatalytic nitrogen fixation catalyst

By loading Ni single atomic load on the ZnO@NC heterojunction, the problem of low nitrogen reduction efficiency of photocatalytic nitrogen fixing catalysts at room temperature and pressure is solved, and high-efficiency nitrogen reduction synthesis is achieved, thereby improving the photometric The efficiency and stability of catalytic nitrogen fixation reaction have the advantages of green environmental protection and low cost.

CN116037183BActive Publication Date: 2024-11-26GUANGZHOU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211540418.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-11-26
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

The existing photocatalytic nitrogen fixing catalysts have low efficiency in synthesis of ammonia at normal temperature and pressure, and lack effective nitrogen activation sites, resulting in slow kinetics of the reduction reaction and low photocatalytic efficiency.

Method used

By loading precursor metal clusters, Ni single atoms of single-core and dual-core sites are loaded on the ZnO@NC heterojunction to form a ZnO@NC-Ni2 catalyst, providing rich active sites and high-efficiency electron mobility , overcome the problems of low photogenerated electron reduction ability and high recombination rate.

Benefits of technology

It achieves efficient nitrogen reduction and synthesis of ammonia, improves the efficiency and stability of photocatalytic nitrogen fixation reaction, overcomes the problems of insufficient active sites of the original catalyst and the prone to falling off metal sites, and has the advantages of green and environmental protection and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116037183B_ABST
    Figure CN116037183B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of optoelectronic energy materials, and discloses a method for preparing a high-performance photocatalytic nitrogen fixation catalyst, which realizes the synthesis of ammonia by nitrogen reduction at room temperature and pressure through a photocatalytic method. In order to further improve its performance, Ni single atoms at mononuclear and binuclear sites are loaded on ZnO@NC heterojunctions by a method of loading precursor metal clusters. After experimental exploration, it is found that ZnO@NC‑Ni2 has the best performance. The catalyst overcomes the problems of low reduction ability of photogenerated electrons and high recombination rate of photogenerated carriers, and at the same time, forms side-end bridging adsorption with N2 through its special binuclear active sites, thereby achieving an effective adsorption process (chemical adsorption) of N2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photoelectric energy materials, and in particular to a method for preparing a high-performance photocatalytic nitrogen fixation catalyst. Background Art

[0002] Ammonia (NH3) is the main chemical raw material in the fertilizer industry and an important carbon-free energy carrier. Natural nitrogen fixation methods such as nitrogenase in biochemistry and lightning nitrogen fixation in geochemistry, and naturally produced ammonia are far from meeting the needs of human social development. At present, the production of NH3 relies on the energy-intensive Haber-Bosch process. However, the Haber-Bosch process, which uses H2 gas (mainly obtained through steam reforming) as a raw material, requires huge energy consumption and will cause a large amount of greenhouse gas emissions. According to statistics, the Haber-Bosch process consumes 1-2% of the global energy supply and produces about 3% of the total global carbon dioxide emissions. (Nat. Catal., 2019, 2, 1055.) 1, resulting in a large amount of energy consumption and greenhouse gas emissions. Industrial ammonia synthesis technology, an energy-intensive industry, urgently needs to be transformed and upgraded because it consumes a lot of resources and energy and emits greenhouse gases that pollute the environment. Therefore, scientists have been looking for new ways to make the way of synthesizing ammonia greener and more sustainable. Photocatalytic nitrogen fixation to synthesize NH3 is a semiconductor photocatalyst that utilizes abundant N2, H2O, and solar energy to achieve the synthesis of NH3 at room temperature and pressure, opening up a new direction for solving energy shortages, climate warming, and environmental sustainability.

[0003] The photocatalytic nitrogen reduction reaction (pNRR) is an alternative to the energy-intensive Haber-Bosch process and has attracted widespread attention due to its energy-saving and environmentally friendly advantages. Despite the numerous advantages of photocatalytic nitrogen fixation, breakthroughs in effective photocatalytic nitrogen fixation have rarely been achieved in the past few years due to the lack of effective active centers in the core catalysts to bind and crack nitrogen. In order to solve the problems of photocatalytic nitrogen fixation in this regard, it is an important and challenging topic to construct green and sustainable photocatalysts with abundant active sites to achieve a reliable photocatalytic nitrogen fixation pathway.

[0004] Although some substantial progress has been made in photocatalytic nitrogen fixation, several aspects of the photocatalytic nitrogen fixation pathway must be resolved before it can generate practical value. First, the nitrogen reduction reaction (NRR) and hydrogen evolution reaction (HER) have similar reduction potentials, so the selectivity for NRR is reduced in aqueous electrolytes, favoring HER. Second, the stable N≡N molecules lack suitable adsorption and activation sites on the photocatalyst surface, resulting in sluggish NRR kinetics. In addition, the high recombination rate of photogenerated carriers and poor visible light capture ability lead to low overall photocatalytic nitrogen fixation efficiency. In general, since single-component photocatalysts are usually inefficient, several strategies have been developed to improve the photoactivity of photocatalysts. These strategies include the loading of co-catalysts, the introduction of defects, and the formation of heterojunctions. Heterojunction-based photocatalysts currently have the highest potential for enhancing photocatalytic activity due to the charge transfer mechanism and separation of photogenerated carriers, which is a key issue in solving the low efficiency of single-component photocatalysts. Therefore, constructing green and sustainable semiconductor photocatalysts with abundant active sites and efficient electron mobility to achieve efficient photocatalytic ammonia synthesis remains an important and challenging topic. As we all know, ZnO@NC heterojunction is a new type of photocatalyst with the advantages of low cost, high photostability, non-toxicity and environmental friendliness. However, although ZnO@NC heterojunction semiconductor is not a single component, it lacks effective nitrogen activation sites, making it difficult to achieve efficient nitrogen fixation using renewable solar energy.

[0005] Of course, materials of plasma metal-loaded semiconductor oxides, such as Au, Pt / TiO2, Au / CdS and other photocatalysts have been widely studied. However, the metal sites of these catalysts are mostly either wrapped by carrier oxides, resulting in fewer effective active sites on the surface, or are not firmly bonded to the substrate, resulting in easy detachment. These will greatly reduce the photocatalytic activity. For this reason, we proposed a method for preparing a high-performance photocatalytic nitrogen fixation catalyst. Summary of the invention

[0006] 1. Technical issues to be resolved

[0007] In view of the shortcomings of the prior art, the present invention provides a method for preparing a high-performance photocatalytic nitrogen fixation catalyst, which realizes the synthesis of ammonia by nitrogen reduction at room temperature and pressure through a photocatalytic method. In order to further improve its performance, the Ni single atoms of mononuclear and binuclear sites are loaded on the ZnO@NC heterojunction by loading the precursor metal cluster. After experimental investigation, it is found that ZnO@NC-Ni2 has the best performance. The catalyst overcomes the problems of low reduction ability of photogenerated electrons and high recombination rate of photogenerated carriers, and at the same time, through its special binuclear active sites, it forms a side-bridge adsorption with N2, thereby achieving an effective adsorption process of N2.

[0008] (II) Technical solution

[0009] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a method for preparing a high-performance photocatalytic nitrogen fixation catalyst, comprising the following steps:

[0010] Step 1: Dissolve zinc nitrate in methanol, then add 2-methylimidazole, stir at room temperature, centrifuge the resulting precipitate, wash three times with methanol, and vacuum dry overnight to obtain white ZIF-8 powder. Heat ZIF-8 and cool to room temperature to obtain ZnO@NC powder.

[0011] Step 2: First, place the reaction system in an ice-water bath and degas at room temperature, then add deoxygenated tetrahydrofuran into the bottle, add nickel chloride hexahydrate into the above solution, add methanol, stir, then add bis(diphenylphosphine)methane into the Shrek bottle, add sodium borohydride into the Shrek bottle, react, and obtain Ni2(dppm)2Cl3 cluster compound;

[0012] Step 3: Disperse ZnO@NC in dichloromethane, ultrasonicate, dropwise add dichloromethane solution containing Ni2(dppm)2Cl3 into the above solution, vigorously stir at room temperature, centrifuge the obtained precipitate, dry overnight in vacuum, place the dried sample in a corundum ark, heat it, and finally obtain ZnO@NC-Ni2;

[0013] Step 4: Using Ni(1,3-bis(diphenylphosphino)propane)2 as a precursor, repeat the third step to obtain the ZnO@NC-Ni1 catalyst.

[0014] Preferably, in the first step, the zinc nitrate is 0.87 g, the methanol is 30 mL, and the 2-methylimidazole is 1.97 g;

[0015] The stirring time is 12h;

[0016] Vacuum drying overnight at 60°C;

[0017] The heating condition was heating at 500° C. for 2 hours at a heating rate of 2° C. / min in a muffle furnace.

[0018] Preferably, the degassing time in the second step is 20 min, the amount of deoxytetrahydrofuran added is 50 ml, the amount of nickel chloride hexahydrate added is 240 mg, the amount of methanol added is 5 ml, the amount of bis(diphenylphosphino)methane added is 600 mg, and the amount of sodium borohydride added is 80 mg;

[0019] The stirring time is 5 minutes;

[0020] The time of adding sodium borohydride is 30 minutes after adding bis(diphenylphosphino)methane;

[0021] The reaction time after adding sodium borohydride was 4 hours.

[0022] Preferably, the synthesis process in the third step should be strictly carried out in an Ar gas atmosphere.

[0023] Preferably, in the third step, the amount of ZnO@NC added is 400 mg, the amount of dichloromethane is 30 mL, the amount of dichloromethane solution is 20 mL, and the amount of dichloromethane solution contains 20 mg Ni2(dppm)2Cl3;

[0024] The ultrasonic time was 30 min, the vigorous stirring time was 12 h, and the temperature for drying overnight in vacuum was 60 °C;

[0025] The heating conditions were heating at 400° C. for 2 hours at a heating rate of 5° C. / min.

[0026] (III) Beneficial effects

[0027] Compared with the prior art, the present invention provides a method for preparing a high-performance photocatalytic nitrogen fixation catalyst, which has the following beneficial effects:

[0028] 1. The preparation method of this high-performance photocatalytic nitrogen fixation catalyst, the green and environmentally friendly ZnO@NC-Ni2 photocatalyst, can fundamentally realize the synthesis of ammonia by N2 reduction at room temperature and pressure through photocatalytic methods. It effectively overcomes the problems of low efficiency of ZnO@NC photocatalytic reduction of N2, low reduction ability of photogenerated electrons, and high recombination rate of photogenerated carriers.

[0029] 2. Preparation method of the high-performance photocatalytic nitrogen fixation catalyst. ZnO@NC heterojunction has the advantages of wide visible light response, high photostability, and environmental friendliness, and is a promising pNRR catalyst. However, in the ZnO@NC heterojunction material, the reduction ability of its photogenerated electrons is low, and an effective pNRR reaction cannot occur. In addition, the high recombination rate of photogenerated electrons and holes hinders its wide application in pNRR. Therefore, in order to improve the pNRR activity of the ZnO@NC heterojunction, it is combined with Ni metal clusters to become a single-atom supported catalyst, which provides a large number of active centers, can effectively activate N2, and enhance the transmission and separation efficiency of photogenerated electrons and holes, so as to achieve the purpose of improving the pNRR activity. It effectively overcomes the disadvantages of easy deactivation of sites and easy detachment of loaded metal nanoparticles caused by methods such as modifying oxygen vacancies (OVs) and heteroatoms.

[0030] 3. The preparation method of this high-performance photocatalytic nitrogen fixation catalyst has a simple synthesis process. Due to the characteristics of low single-atom catalyst content and high atomic utilization, it can reduce costs and is expected to be used for industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1Transmission electron microscope image of ZnO@NC;

[0032] Figure 2 HAADF-STEM image of ZnO@NC-Ni2 (b). HAADF-STEM corresponding EDS mapping (c) and high-resolution TEM (a) image of ZnO@NC-Ni2;

[0033] Figure 3 TEM image (a), HAADF-STEM image (b), and corresponding EDS mapping (c) of ZnO@NC-Ni1;

[0034] Figure 4 X-ray diffraction (XRD) tests were performed using a PANalytical X'Pert PRO instrument with Cu Kα radiation;

[0035] Figure 5 The nitrogen adsorption of ZnO@NC, ZnO@NC-Ni1 and ZnO@NC-Ni2 was studied by temperature-programmed nitrogen desorption (TPD) experiment.

[0036] Figure 6 For PL spectrum test, the recombination of photogenerated carriers of ZnO@NC, ZnO@NC-Ni1 and ZnO@NC-Ni2 was investigated;

[0037] Figure 7 (a) XANES spectrum of Ni k-edge. (b) Fourier transform (FT) of Ni EXAFS edge EXAFS. (c) FT of R-space EXAFS spectrum.

[0038] Figure 8 XPS spectra of Zn2p (a), O1s (b), C1s (c), N1s (d) and Ni2p (f) in ZnO@NC, ZnO@NC-Ni1 and ZnO@NC-Ni2;

[0039] Fig. 9 The photocatalytic ammonia synthesis yield of ZnO@NC, ZnO@NC-Ni1 and ZnO@NC-Ni2 catalysts under light irradiation;

[0040] Fig.10 Cyclic test of ZnO@NC-Ni2. (The reaction was tested for 2 h in each cycle). DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The materials and chemicals involved in the following examples and comparative examples include: nickel (II) chloride hexahydrate (NiCl2·6H2O), zinc nitrate, sodium borohydride (sodium borohydride), 2-methylimidazole, bis(diphenylphosphino)methane, sodium borohydride, methanol, tetrahydrofuran (THF), 1,3-bis(diphenylphosphino)propane, dichloromethane and 2-methylimidazole (MeIM) were purchased from Beijing Nuo Chemical Reagent Co., Ltd. All chemicals were of analytical purity (AR) and did not require further purification.

[0043] The characterization instruments used in the following examples and comparative examples are as follows: The samples were characterized by different analytical techniques. The catalysts were characterized by powder x-ray diffraction (XRD, Philips X'pertPRO x-ray diffractometer, Cu Kα, λ=1.54182A), scanning electron microscopy (SEM, FEI-30ESEM) and transmission electron microscopy (TEM, Hitachi H-7700). High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) was performed on a JEOL JEM-ARF200FTEM / STEM. EDS elemental mapping was obtained on a 26FEI Talos F200X instrument. The absorption spectrum was analyzed by diffuse reflectance spectroscopy (DRS, HITACHI UV-3900). The photochemical reactor was installed on a CEL-GPPcL system (Beijing China Education Optoelectronics Co., Ltd.) and equipped with a 300-W Xe lamp. Chemical adsorption of N2 was performed in a N2 temperature-programmed desorption experiment (Microparticle Automation Chemistry II) using TCD as a detector. The surface electronic states were analyzed by X-ray photoelectron spectroscopy (XPS, Thermoscalab250Xi), and all binding energies were referenced to the C1s peak at 284.8 eV. The steady-state and transient photoluminescence (PL) curves of the material were excited by a hydrogen flash lamp with an excitation wavelength of 800 nm. Raman spectra were recorded on a HORIBA Xplora Plus spectrometer using a 532 nm Ar laser. The content of Ni loaded on ZnO@NC was determined by inductively coupled plasma optical emission spectrometry (ICP-OES, PerkinElmer).

[0044] Example

[0045] (1) Preparation of ZnO@NC:

[0046] 0.87 g of zinc nitrate was dissolved in 30 mL of methanol, and then added to 30 mL of methanol containing 1.97 g of 2-methylimidazole (MeIM) and stirred at room temperature for 12 h. Next, the resulting precipitate was centrifuged and washed three times with methanol. After vacuum drying at 60 ° C overnight, white ZIF-8 powder was obtained. The prepared ZIF-8 was heated at 500 ° C for 2 hours in a muffle furnace at a heating rate of 2 ° C / min. After the temperature was cooled to room temperature, ZnO@NC powder was obtained.

[0047] (2) Synthesis of Ni2(dppm)2Cl3 cluster compound: First, place the reaction system in an ice-water bath, degas 100 ml of the solution at room temperature for 20 min, and then add 50 ml of deoxygenated tetrahydrofuran into the bottle. Then, add 240 mg of nickel chloride hexahydrate to the above solution, add 5 ml of methanol, stir for 5 min, and then add 600 mg of bis(diphenylphosphine)methane into the Shrek bottle. After 30 minutes, add 80 mg of sodium borohydride into the Shrek bottle, react for 4 hours, and obtain the purified product.

[0048] (3) Synthesis of ZnO@NC-Ni2 catalyst: Ni2(dppm)2Cl3 clusters are very sensitive to oxygen, and the synthesis process should be strictly carried out in an Ar atmosphere. 400 mg ZnO@NC was dispersed in 30 mL dichloromethane and ultrasonicated for 30 min. Then, 20 mL of dichloromethane solution containing 20 mg Ni2(dppm)2Cl3 clusters was added dropwise to the above system and stirred vigorously at room temperature for 12 h. Then, the obtained precipitate was centrifuged and dried in a vacuum at 60 °C overnight. The dried sample was placed in a corundum ark and heated at 400 °C for 2 h in an Ar atmosphere at a heating rate of 5 °C / min. The final product was stored in a glass bottle for later use.

[0049] (4) Synthesis of ZnO@NC-Ni1 catalyst: It was synthesized in a similar way to ZnO@NC-Ni2, using Ni(1,3-bis(diphenylphosphino)propane)2 as the precursor.

[0050] Experimental data

[0051] Material characterization and performance testing:

[0052] 1. Photocatalytic nitrogen fixation reaction process

[0053] Photocatalytic nitrogen fixation and ammonia synthesis experiments were carried out on a self-assembled photocatalytic reaction platform. Photocatalytic nitrogen fixation was achieved at the three-phase interface (gas phase N2, liquid phase H2O and solid phase photocatalyst) at room temperature and normal pressure. The light source used was a 300w xenon lamp (full spectrum), and the light source was 10cm away from the liquid surface. The specific experimental steps are as follows: First, 20mg of the ZnO@NC-Ni photocatalyst prepared in Example 1 was dispersed in 50mL of deionized water and added to a reactor with a circulating water system. Secondly, high-purity N2 (200mL min -1 ) and stirred continuously for 30 minutes to saturate the aqueous solution with N2. Then, light was applied, and 4.0 mL of the reaction solution was taken out every 30 minutes and filtered through a 0.22 μm filter to detect the content of synthetic ammonia.

[0054] 2. Detection method of ammonium ions in aqueous solution:

[0055] The ammonia content in the photocatalytic reaction solution was detected by the indophenol blue method. Take 2.0 mL of the above mixed solution, add 0.5 mL of phenol nitroprusside solution and 0.5 mL of alkaline sodium hypochlorite solution, and incubate for 30 minutes at room temperature in the dark. Use UV-visible spectroscopy (UV-17800, Shimadzu) to test the absorbance of the unmixed sample, and calculate the actual yield based on the established standard curve.

[0056] 3. The Ni metal content in ZnO@NC-Ni1 and ZnO@NC-Ni2 was determined by inductively coupled plasma spectroscopy (ICP-OES), and the ratio of the Ni metal content to the loading content was basically consistent, indicating that the preparation method of the present invention is stable and effective.

[0057] 4. Use transmission electron microscopy (TEM) to perform physical characterization on ZnO@NC, ZnO@NC-Ni1, and ZnO@NC-Ni2 to obtain the morphology of the corresponding catalysts. EDS shows that the Ni unit is uniformly loaded on the substrate, and no corresponding peak appears in the XRD spectrum, indicating that the corresponding single-atom catalyst has been synthesized.

[0058] 5. Using PANalytical X'Pert PRO instrument and Cu Kα radiation, X-ray diffraction (XRD) tests were performed on ZnO@NC, ZnO@NC-Ni1, and ZnO@NC-Ni2.

[0059] 6. Using the temperature programmed nitrogen desorption (TPD) experiment ( Figure 3) Comparison of chemical adsorption of N2 on ZnO@NC, ZnO@NC-Ni1, and ZnO@NC-Ni2 was performed, and the role of the catalyst in the effective N2 activation site of the photocatalytic nitrogen reduction reaction was evaluated through different responses. Simply put, the higher the high-temperature desorption front signal, the more favorable it is for the chemical adsorption of N2 on the catalyst surface, the more favorable it is for weakening the nitrogen-nitrogen triple bond, and the easier it is for the photocatalytic reduction of N2 to NH3, thus having a higher photocatalytic activity. Figure 4 As shown in , compared with unloaded ZnO@NC, ZnO@NC-Ni2 loaded with Ni single atoms can more effectively adsorb N2 molecules, indicating that its photocatalytic reduction activity is optimal, confirming the advantage of the present invention in preparing synthetic materials to optimize pNRR activity.

[0060] 7. Through the steady-state and transient photoluminescence (PL) curve tests of the material, the more the photogenerated carriers of the material recombine, the stronger its fluorescence intensity. The fluorescence intensity of ZnO@NC-Ni2 synthesized by the present invention is the lowest compared with ZnO@NC and ZnO@NC-Ni1, indicating that its photogenerated carrier load rate is low and it can have a higher electron mobility to promote the photocatalytic nitrogen fixation reaction.

[0061] 8. To further investigate the chemical state and coordination structure of Ni in ZnO@NC-Ni2, we conducted X-ray absorption near-edge structure (XANES) and extended X-ray absorption fine structure (EXAFS) spectroscopy studies ( Figure 7 ) and XPS test ( Figure 8 ), and the corresponding coordination structure of Ni and the chemical states of C, N, O, and Zn elements were obtained.

[0062] 9. Next, the ZnO@NC-Ni2 material prepared by the present invention was subjected to a photocatalytic nitrogen reduction cycle test. The results are as follows: Figure 5 As shown in the figure, after five cycles of testing, its activity remained basically unchanged, and its performance in synthesizing ammonia did not decrease significantly. This confirms that the structure of the ZnO@NC-Ni2 material has excellent light stability, indicating that the method of the present invention effectively overcomes the disadvantages of methods such as modifying oxygen vacancies (OVs) and metal nanoparticles, which are prone to photocorrosion and easy to fall off, resulting in easy inactivation of the site.

[0063] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An application of a photocatalytic nitrogen fixation catalyst, characterized in that: The preparation method of the photocatalytic nitrogen fixation catalyst comprises the following steps: Step 1: Dissolve zinc nitrate in methanol, then add 2-methylimidazole, stir at room temperature, centrifuge the resulting precipitate, wash three times with methanol, and vacuum dry overnight to obtain white ZIF-8 powder. Heat ZIF-8 and cool to room temperature to obtain ZnO@NC powder. Step 2: First, place the reaction system in an ice-water bath and degas at room temperature, then add deoxygenated tetrahydrofuran into the bottle, add nickel chloride hexahydrate into the above solution, add methanol, stir, then add bis(diphenylphosphine)methane into the Shrek bottle, add sodium borohydride into the Shrek bottle, react, and obtain Ni2(dppm)2Cl3 cluster compound; Step 3: Disperse the ZnO@NC powder obtained in the first step in dichloromethane, perform ultrasound, dropwise add a dichloromethane solution containing Ni2(dppm)2Cl3 into the above solution, vigorously stir at room temperature, centrifuge the obtained precipitate, dry overnight in vacuum, place the dried sample in a corundum ark, and heat it to finally obtain a ZnO@NC-Ni2 photocatalytic nitrogen fixation catalyst in which a single Ni atom at a binuclear site is loaded on a ZnO@NC heterojunction; the photocatalytic nitrogen fixation is to synthesize ammonia by photocatalytic nitrogen reduction on the photocatalytic nitrogen fixation catalyst ZnO@NC-Ni2 at room temperature and pressure.

2. The use of a photocatalytic nitrogen fixation catalyst according to claim 1, characterized in that: In the first step, the zinc nitrate is 0.87 g, the methanol is 30 mL, and the 2-methylimidazole is 1.97 g; The stirring time is 12h; Vacuum drying overnight at 60°C; The heating conditions were heating at 500° C. for 2 hours at a heating rate of 2° C. / min in a muffle furnace.

3. The use of a photocatalytic nitrogen fixation catalyst according to claim 1, characterized in that: The degassing time in the second step is 20 min, the amount of deoxygenated tetrahydrofuran added is 50 ml, the amount of nickel chloride hexahydrate added is 240 mg, the amount of methanol added is 5 ml, the amount of bis(diphenylphosphino)methane added is 600 mg, and the amount of sodium borohydride added is 80 mg; The stirring time is 5 min; The sodium borohydride was added 30 minutes after the addition of bis(diphenylphosphino)methane; The reaction time after adding sodium borohydride was 4 hours.

4. The use of a photocatalytic nitrogen fixation catalyst according to claim 1, characterized in that: The synthesis process in the third step is strictly carried out in an Ar gas atmosphere.

5. The use of a photocatalytic nitrogen fixation catalyst according to claim 1, characterized in that: In the third step, the amount of ZnO@NC powder added is 400 mg, the amount of dichloromethane is 30 mL, the amount of dichloromethane solution containing Ni2(dppm)2Cl3 is 20 mL, and the amount of dichloromethane solution containing Ni2(dppm)2Cl3 is 20 mg; The ultrasonic time was 30 min, the vigorous stirring time was 12 h, and the temperature for drying overnight in vacuum was 60 °C; The heating conditions were heating at 400° C. for 2 hours at a heating rate of 5° C. / min.