A carbon-coated iron-cobalt bimetallic nanoparticle catalyst for Friedel-Crafts acylation reaction and a preparation method thereof
The carbon-coated iron-cobalt bimetallic nanoparticle catalyst was prepared by co-precipitation method and programmed temperature pyrolysis reaction, which solved the problems of large dosage of traditional catalyst and complicated preparation process, achieved high activity and stability in Friedel-Crafts acylation reaction, and promoted Catalyst recycling.
Patent Information
- Application Number
- CN202211736674.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-31
AI Technical Summary
The Lewis acid catalyst used in the traditional Friedel-Crafts acylation reaction has problems such as large catalyst dosage, difficulty in separation from the product, inability to be recycled, and strong corrosiveness. In addition, the preparation process of existing carbon-coated metal nanomaterials is complex, poor safety, and costly. High and difficult to adapt to large-scale production.
The iron-cobalt-based Prussian blue analogue Co3[Fe(CN)6]2 was prepared by co-precipitation method, and melamine was used as an auxiliary carbon source and nitrogen source to perform a temperature-programmed pyrolysis reaction to prepare carbon-coated iron-cobalt bimetallic nanometers. The particle catalyst ensures that the iron-cobalt bimetallic nanoparticles are evenly distributed on the carbon carrier to form a uniform graphite carbon layer, improving the cycle stability and catalytic activity of the catalyst.
It achieves high catalytic activity and stability under harsh reaction conditions, facilitates catalyst recycling, reduces preparation costs and process complexity, and is suitable for Friedel-Crafts acylation reactions.
Smart Images

Figure CN116037186B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heterogeneous catalysis, and in particular relates to a carbon-coated iron-cobalt bimetallic nanoparticle catalyst for Friedel-Crafts acylation reaction and a preparation method thereof. Background Art
[0002] The main method for preparing aromatic ketone compounds is to carry out Friedel-Crafts acylation reaction with aromatic hydrocarbons and acyl chlorides (or anhydrides) as reaction substrates under the action of acid catalysts. However, the traditional process requires the use of stoichiometric amounts of Lewis acids such as AlCl3 or FeCl3 as homogeneous catalysts, which have the problems of large catalyst dosage, difficulty in separation from the product, inability to recycle, and easy corrosion of equipment and high environmental pressure. In order to overcome the above problems, researchers have been committed to the research and development of efficient heterogeneous catalysts with excellent catalytic performance and easy recycling.
[0003] In recent years, a class of carbon-coated metal nanomaterials prepared by high-temperature pyrolysis of metal organic frameworks (MOFs) has attracted widespread attention. This type of material has a large specific surface area, good electrical conductivity, and high structural stability, and shows good application prospects in the fields of heterogeneous catalysis and electrocatalysis (Juntao Tang, Jianlong Wang, Chemical Engineering Journal 375 (2019) 122007; Limin Zhou, Jing Meng et al, Mater. Horiz., 2017, 4, 268). Hao Zhang et al. used an organic solvent thermal method to synthesize a type of Fe-MOFs precursor constructed of triethylenediammonium and iron ions, and then prepared a nitrogen-doped carbon-coated iron-based nanoparticle Fe@NC catalyst by high-temperature pyrolysis. The catalyst can effectively catalyze the Friedel-Crafts acylation reaction of various aromatic hydrocarbons with acyl chlorides and has good cyclic stability (CN109772406B; H. Zhang, M. Jia et al, Catal. Sci. Technol., 2019, 9, 3812-3819); Chen Zhao et al. used terephthalic acid as an organic ligand, melamine as an auxiliary nitrogen source and carbon source, and N,N-dimethylformamide as a solvent to synthesize a type of Fe-MOFs material, and then prepared a nitrogen-doped carbon-coated iron nanoparticle catalyst Fe / C by high-temperature pyrolysis. The catalyst can also be used as an effective Friedel-Crafts acylation reaction heterogeneous catalyst. However, in the process of synthesizing Fe-MOFs precursors, the above-mentioned catalysts all require the use of a large amount of organic solvents and relatively expensive organic nitrogen-containing ligands, and the use of higher reaction temperatures in autoclaves for solvothermal reactions, resulting in complex catalyst preparation processes, poor safety, high costs, and other issues, which are not conducive to large-scale production and application.
[0004] As a class of MOFs materials with unique structure, Prussian blue (PB) and its analogs (PBAs) have the advantages of simple synthesis method, easy adjustment of composition structure, and can be synthesized in water system under mild conditions. They can also be used to prepare various nitrogen-doped carbon-based metal nanomaterials. For example, Cai et al. synthesized nitrogen-doped graphitic carbon-coated bimetallic nanomaterials FeCo@NC by pyrolysis of PBA with composition Co3[Fe(CN)6]2. The two metal components in the material can form an alloy phase and can be used as an active and stable catalyst in electrocatalytic oxygen production reaction (P. Cai et al. Electrochimica Acta, 2016, 220, 354-362). However, compared with other types of MOFs materials, carbon-based metal nanoparticle catalysts prepared with PBA as a precursor generally have uneven distribution of metal components, which are easy to aggregate into large metal particles, resulting in low utilization of active metal components of the catalyst, and it is difficult to maintain high stability under harsh reaction conditions (M. Zhang, C. Wang, R. Luo, W. Zhang, S. Chen, X. Yan, J. Qi, X. Sun, L. Wang, J. Li, J. Mater. Chem. A, 2019, 7, 5173-5178). For the Friedel-Crafts acylation reaction, whether PBAs can be used as precursors to optimize various preparation parameters to obtain economical and practical carbon-based transition metal catalysts with excellent performance is still an important problem to be solved in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a carbon-coated iron-cobalt bimetallic nanoparticle catalyst on the basis of the prior art. The invention comprises the following steps: firstly, a coprecipitation method is adopted to prepare an iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2 (denoted as PBA-FeCo) with polyvinyl pyrrolidone (PVP) as a growth regulator; melamine is used as an auxiliary carbon source and nitrogen source, mixed with melamine, and ground to obtain a pyrolysis precursor (denoted as PBA-FeCo / Xm); then a programmed temperature pyrolysis reaction (step-by-step pyrolysis reaction) is carried out in an inert atmosphere to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst (denoted as FeCo-Xm / NC-T); in the catalyst, the iron-cobalt bimetallic nanoparticles are evenly distributed on a carbon carrier, and the thickness of the formed carbon-coated graphite carbon layer is even, which can provide effective protection for the iron-cobalt bimetallic nanoparticles in the shell, so that the catalyst can maintain high catalytic Friedel-Crafts acylation reaction activity and stability under relatively harsh reaction conditions, is easy to recycle, and has relatively excellent cycle performance.
[0006] Another object of the present invention is to provide a method for preparing the above-mentioned carbon-coated iron-cobalt bimetallic nanoparticle catalyst. The preparation method is simple, the conditions are mild, and the cost is low. The prepared carbon-coated iron-cobalt bimetallic nanoparticle catalyst has a stable structure, high catalytic activity, can be recycled multiple times, and is particularly suitable for Friedel-Crafts acylation reaction.
[0007] The third object of the present invention is to provide the use of the above catalyst as a catalyst in Friedel-Crafts acylation reaction.
[0008] The technical solution of the present invention is as follows:
[0009] A carbon-coated iron-cobalt bimetallic nanoparticle catalyst is prepared by pyrolysis of a mixture of an iron-cobalt-based Prussian blue analogue and melamine, comprising iron-cobalt bimetallic nanoparticles and a graphite carbon layer, wherein the surface of the iron-cobalt bimetallic nanoparticles is coated with the graphite carbon layer, wherein the particle size of the iron-cobalt bimetallic nanoparticles is 10 to 90 nm; and the thickness of the graphite carbon layer is 1 to 10 nm.
[0010] In a preferred embodiment, in the carbon-coated iron-cobalt bimetallic nanoparticle catalyst, the total content of iron and cobalt bimetallic is 30-80wt%, wherein the molar ratio of iron to cobalt is 2:3; the specific surface area of the catalyst is 20-60m 2 / g.
[0011] The carbon-coated iron-cobalt bimetallic nanoparticle catalyst mentioned in the present invention is prepared by the following steps:
[0012] (1) Cobalt salt CoSO4·7H2O, polyvinyl pyrrolidone and water are mixed uniformly, K3[Fe(CN)6] is added to the obtained mixed solution and stirred uniformly, and then an aging reaction is carried out at room temperature. The obtained reaction solution is centrifuged, washed with water, and dried to obtain an iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2, which is recorded as PBA-FeCo;
[0013] (2) uniformly mixing melamine with the iron-cobalt-based Prussian blue analogue obtained in step (1) to obtain a pyrolysis precursor, denoted as PBA-FeCo / Xm; wherein the mass ratio of melamine to the iron-cobalt-based Prussian blue analogue is 1 to 15:1;
[0014] (3) The pyrolysis precursor obtained in step (2) is subjected to a programmed temperature pyrolysis reaction in an inert atmosphere to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst, denoted as FeCo-Xm / NC-T; wherein the programmed temperature pyrolysis procedure is: heating to 550°C at a heating rate of 1 to 5°C / min, maintaining for 1 to 3 hours, and then heating to 600 to 1000°C at a heating rate of 1 to 5°C / min and maintaining for 1 to 4 hours.
[0015] In a preferred embodiment, in step (1), the mass ratio of the cobalt salt CoSO4·7H2O to polyvinyl pyrrolidone is 0.3 to 0.8:1, and can be but not limited to 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1 or 0.8:1. In order to obtain better results, the mass ratio of the cobalt salt CoSO4·7H2O to polyvinyl pyrrolidone is 0.5:1.
[0016] In a preferred embodiment, in step (1), the molar ratio of the cobalt salt CoSO4·7H2O to K3[Fe(CN)6] is 1.0 to 2.0:1, and can be but not limited to 1.0:1, 1.2:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1 or 2.0:1. In order to obtain better results, the molar ratio of the cobalt salt CoSO4·7H2O to K3[Fe(CN)6] is 1.5:1.
[0017] In step (1), the aging reaction time is 20 to 30 hours, preferably 24 hours.
[0018] In step (1), the drying temperature is 70-90°C, and may be but is not limited to 70°C, 75°C, 80°C, 85°C or 90°C. To obtain better effects, the drying temperature is 80°C.
[0019] In the present invention, in step (2), the mass ratio of melamine to the iron-cobalt-based Prussian blue analogue is 1 to 15:1, and may be but not limited to 1:1, 3:1, 5:1, 8:1, 10:1 or 15:1. In order to obtain better effects, the mass ratio of melamine to the iron-cobalt-based Prussian blue analogue is 1:1, 5:1 or 10:1. More preferably, the mass ratio of melamine to the iron-cobalt-based Prussian blue analogue is 5:1.
[0020] In a preferred embodiment, in step (3), the programmed temperature pyrolysis program is: heating to 550°C at a heating rate of 3°C / min, maintaining for 2 hours, and then heating to 600-800°C at a heating rate of 3°C / min, maintaining for 3 hours. For example, the temperature of the second heating can be 600°C, 650°C, 700°C, 750°C or 800°C.
[0021] The carbon-coated iron-cobalt bimetallic nanoparticle catalyst mentioned in the present invention can be prepared by the following more detailed steps:
[0022] (1) 1.5 mmol CoSO4·7H2O and 0.8 g polyvinylpyrrolidone (PVP) were dissolved in 80 mL water, and 80 mL of aqueous solution containing 1.0 mmol K3[Fe(CN)6] was added under continuous stirring, and the mixture was stirred and aged for 24 h. The precipitate generated in the reaction was then centrifuged, washed with water, and dried at 80°C to obtain a brick-red solid powder, which was the iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2 (denoted as PBA-FeCo).
[0023] (2) uniformly mixing melamine (denoted as m) and the iron-cobalt-based Prussian blue analog (PBA-FeCo) obtained in step (1), and grinding to obtain a pyrolysis precursor, denoted as PBA-FeCo / Xm; wherein the mass ratio of melamine (denoted as m) to the iron-cobalt-based Prussian blue analog (PBA-FeCo) is X:1; wherein X=1, 5, 10;
[0024] (3) subjecting the pyrolysis precursor PBA-FeCo / Xm obtained in step (2) to a programmed temperature pyrolysis reaction in an inert atmosphere to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst, denoted as FeCo-Xm / NC-T; wherein the programmed temperature pyrolysis procedure is: heating to 550°C at a heating rate of 1 to 5°C / min, maintaining for 1 to 3 hours, and then heating to the pyrolysis reaction temperature T at a heating rate of 1 to 5°C / min, maintaining for 1 to 4 hours; wherein the pyrolysis reaction temperature T is 600 to 1000°C, and can be 600°C, 650°C, 700°C, 750°C, 800°C, 900°C or 1000°C; preferably, the pyrolysis reaction temperature T is 600°C, 700°C or 800°C, and more preferably, the pyrolysis reaction temperature T is 800°C.
[0025] In a preferred embodiment, in step (3), the programmed temperature pyrolysis program is: heating to 550°C at a heating rate of 3°C / min, maintaining for 2 hours, and then heating to 600-800°C at a heating rate of 3°C / min, maintaining for 3 hours. For example, the temperature of the second heating can be 600°C, 650°C, 700°C, 750°C or 800°C.
[0026] The carbon-coated iron-cobalt bimetallic nanoparticle catalyst provided by the present invention can be used in Friedel-Crafts acylation reaction and has high catalytic activity. For example, in the Friedel-Crafts acylation reaction with aromatic hydrocarbons as substrates and acyl chlorides as acylating agents, the conversion rate of acyl chlorides can reach more than 80%.
[0027] In a preferred embodiment, in the Friedel-Crafts acylation reaction with aromatic hydrocarbon as substrate and acyl chloride as acylating agent, the molar ratio of aromatic hydrocarbon to acyl chloride is 1 to 5:1, preferably 2:1; the mass molar ratio of the catalyst to acyl chloride is 40 to 100 mg / mol, preferably 50 mg / mol; the reaction temperature is 90 to 150° C., preferably 130° C.; and the reaction time is 1 to 8 hours.
[0028] The substrate aromatic hydrocarbon mentioned in the present invention may be but is not limited to one or more of toluene, o-xylene, m-xylene, p-xylene, mesitylene, toluene or o-phenylene dimethyl ether. Preferably, the substrate aromatic hydrocarbon is m-xylene, mesitylene or o-phenylene dimethyl ether.
[0029] The acyl chloride mentioned above may be, but is not limited to, one or more of benzoyl chloride, p-methylbenzoyl chloride or p-fluorobenzoyl chloride. Preferably, the acyl chloride is benzoyl chloride.
[0030] Furthermore, the reaction solvent was dodecane. After the reaction was completed, the reaction solution was taken out with a 1 mL syringe, filtered through an organic filter head for multiple times, and then the conversion rate of the reactants and the yield and selectivity of the products were detected by gas chromatography.
[0031] The technical solution of the present invention has the following advantages:
[0032] The invention uses polyvinyl pyrrolidone as a growth regulator, optimizes the reaction conditions for preparing an iron-cobalt-based Prussian blue analog (denoted as PBA-FeCo), adopts melamine as an auxiliary carbon source and a nitrogen source, and adopts a programmed temperature pyrolysis reaction (step-by-step pyrolysis reaction) to prepare a high-efficiency carbon-coated iron-cobalt bimetallic nanoparticle catalyst FeCo-Xm / NC-T suitable for Friedel-Crafts acylation reaction. In particular, the iron-cobalt bimetallic nanoparticles in FeCo-Xm / NC-800 have uniform particle sizes, and the surfaces of the iron-cobalt bimetallic nanoparticles are uniformly coated with a graphite carbon layer, so that the catalyst can maintain high catalytic Friedel-Crafts acylation reaction activity and stability in a strongly acidic environment of the Friedel-Crafts acylation reaction, is easy to recycle, and has relatively excellent cycle performance.
[0033] Compared with other types of catalysts used in Friedel-Crafts acylation reactions, the catalyst of the present invention has the following significant advantages:
[0034] 1) The raw materials for the synthesis of the catalyst are cheap and readily available, the operation steps are simple, and the preparation conditions are mild.
[0035] 2) The carbon-coated iron-cobalt bimetallic nanoparticles in the catalyst have good dispersibility, and the thickness of the carbon-coated graphite carbon layer is uniform.
[0036] 3) The catalyst exhibits high activity, high selectivity and high stability in the Friedel-Crafts acylation reaction of various aromatic hydrocarbons and acyl chlorides. The catalyst can be recovered by simple filtration operation and can be recycled for multiple times. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 : The pyrolysis precursor PBA-FeCo / Xm (wherein X=0, 1, 5, 10) with different melamine ratios in Example 1 of the present invention was pyrolyzed at a pyrolysis reaction temperature of 800° C. to obtain X-ray diffraction patterns of different catalysts FeCo-0m / NC-800, FeCo-1m / NC-800, FeCo-5m / NC-800 and FeCo-10m / NC-800 in turn; wherein FeCo PDF#49-1567 is a standard spectrum belonging to the FeCo alloy phase;
[0038] Figure 2 : Transmission electron microscopy images of catalysts prepared by different pyrolysis methods in Example 2 of the present invention, wherein: Figure 2 Figures a and b are transmission electron microscopy images of the catalyst FeCo-5m / NC at 1 μm and 500 nm, respectively; Figure 2 c and d are transmission electron microscopy images of the catalyst FeCo-5m / NC-800 at 1 μm and 500 nm, respectively;
[0039] Figure 3 : Kinetic curve diagram (a) and cycle experiment diagram (b) of the catalysts FeCo-5m / NC and FeCo-5m / NC-800 prepared by different pyrolysis methods in Friedel-Crafts acylation reaction in Example 2 of the present invention;
[0040] Figure 4 : X-ray diffraction patterns of FeCo-5m / NC-T (T=600, 700 and 800°C) catalysts prepared at different pyrolysis reaction temperatures in Example 3 of the present invention; wherein FeCo PDF#49-1567 is a standard spectrum belonging to the FeCo alloy phase;
[0041] Figure 5 : Scanning electron micrographs of the iron-cobalt-based Prussian blue analogue PBA-FeCo (a), the precursor PBA-FeCo-5m (b), and the catalysts FeCo-5m / NC-550 (c), FeCo-5m / NC-600 (d), FeCo-5m / NC-700 (e), and FeCo-5m / NC-800 (f) obtained by pyrolysis at different temperatures prepared in Example 3 of the present invention;
[0042] Figure 6 : Figure 5 TEM image of FeCo-5m / NC-800(f);
[0043] Figure 7 : Kinetic curve diagram (a) and cycle experiment diagram (b) of the FeCo-5m / NC-T (T=600, 700 and 800°C) catalyst prepared at different pyrolysis reaction temperatures in Example 3 of the present invention in the Friedel-Crafts acylation reaction. DETAILED DESCRIPTION
[0044] In order to more clearly illustrate the present invention, the following are only some examples of the present invention, which are convenient for understanding the specific technical solutions of the present invention, but they do not limit the protection scope of the present invention in any way. All equal changes and modifications made according to the present invention are covered by the patent scope of the present invention. The conversion rate mentioned in the embodiment is the conversion rate of the acyl chloride, and the various substances involved in the reaction and their conversion rates and yields are analyzed by gas chromatography.
[0045] The invention first adopts a coprecipitation method to prepare an iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2 (denoted as PBA-FeCo) with polyvinyl pyrrolidone (PVP) as a growth regulator, adopts melamine as an auxiliary carbon source and nitrogen source, mixes with melamine, grinds to obtain a pyrolysis precursor (denoted as PBA-FeCo / Xm, wherein X=1, 5, 10), and then performs a programmed temperature pyrolysis reaction (step-by-step pyrolysis reaction) in an inert atmosphere to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst (denoted as FeCo-Xm / NC-T, wherein T=600°C, 700°C, 800°C), wherein the particle size of the iron-cobalt bimetallic nanoparticles in the catalyst is 10-90nm; the thickness of the graphite carbon layer is 1-10nm, the total content of the iron and cobalt bimetallic is 30-80wt%, the molar ratio of iron to cobalt is 2:3; the specific surface area of the catalyst is 20-60m 2 / g, and used it for Friedel-Crafts acylation reaction.
[0046] Example 1 Taking the synthesis of FeCo-5m / NC-800 catalyst as an example, the specific preparation method is as follows:
[0047] (1) 1.5 mmol CoSO4·7H2O and 0.8 g polyvinylpyrrolidone (PVP) were dissolved in 80 mL water, and 80 mL of aqueous solution containing 1.0 mmol K3[Fe(CN)6] was added under continuous stirring, and the mixture was stirred and aged for 24 h. The precipitate generated in the reaction was then centrifuged, washed with water, and dried at 80°C to obtain a brick-red solid powder, which was the iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2 (denoted as PBA-FeCo).
[0048] (2) melamine (denoted as m) and the iron-cobalt-based Prussian blue analog (PBA-FeCo) obtained in step (1) are uniformly mixed in a mass ratio of 5:1, and ground to obtain a pyrolysis precursor, denoted as PBA-FeCo / 5m;
[0049] (3) The pyrolysis precursor PBA-FeCo / 5m obtained in step (2) is subjected to a programmed temperature pyrolysis reaction in an inert atmosphere, wherein the programmed temperature pyrolysis program is: heating to 550°C at a heating rate of 3°C / min, maintaining for 2 hours, and then heating to the pyrolysis reaction temperature of 800°C at a heating rate of 3°C / min, maintaining for 3 hours; the obtained product is naturally cooled to room temperature, taken out and ground to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst, recorded as FeCo-5m / NC-800.
[0050] In addition, in step (2), the mass ratio between melamine and the iron-cobalt-based Prussian blue analog (PBA-FeCo) obtained in step (1) is changed to 0:1, 1:1 and 10:1, respectively, to obtain pyrolysis precursors PBA-FeCo / 0m, PBA-FeCo / 1m and PBA-FeCo / 10m with different melamine ratios. Then, the pyrolysis reaction is carried out according to the programmed temperature pyrolysis procedure in step (3), to obtain different catalysts FeCo-0m / NC-800, FeCo-1m / NC-800 and FeCo-10m / NC-800.
[0051] like Figure 1 As shown, the catalysts FeCo-0m / NC-800, FeCo-1m / NC-800, FeCo-5m / NC-800 and FeCo-10m / NC-800 obtained by pyrolysis reaction were characterized by XRD. It can be seen that there are obvious characteristic diffraction peaks at 45°, 65° and 82°, which can be attributed to the FeCo alloy phase (PDF#49-1567). Moreover, with the increase of the amount of melamine introduced, the intensity of the characteristic peak decreases, indicating that the particle size of the iron-cobalt bimetallic nanoparticles is gradually decreasing.
[0052] The Friedel-Crafts acylation performance of the above-mentioned different catalysts was evaluated. The molar ratio of m-xylene to benzoyl chloride was 2:1, the volume of the solvent dodecane was 2.3 mL, the mass of the catalyst FeCo-Xm / NC-800 (X=0, 1, 5, 10) was 50 mg, the reaction temperature was 130°C, and the reaction results are shown in Table 1.
[0053] Table 1 Reaction results of different catalysts in Example 1
[0054] Catalyst name Reaction time / h Conversion rate / % FeCo-0m / NC-800 5 60.8 FeCo-1m / NC-800 5 63.8 FeCo-5m / NC-800 5 81.3 FeCo-10m / NC-800 5 82.9
[0055] As can be seen from Table 1, under the same reaction conditions, when a certain amount of melamine is added (X=1, 5, 10), the catalytic activity is significantly improved; when the addition amount X=5 and 10, the conversion rate of benzoyl chloride is basically maintained at about 81%; the results of the hot filtration experiment show that the catalyst FeCo-5m / NC-800 exhibits good stability, and the recovered catalyst is subjected to multiple cycle experiments and still maintains a high catalytic activity; while a small amount of active species is detected in the FeCo-10m / NC-800 catalyst during the reaction process, indicating that the stability of the catalyst is relatively low and effective recycling cannot be achieved.
[0056] Example 2 uses a FeCo-5m / NC catalyst prepared by one-step heating to 800°C (the pyrolysis platform temperature of 550°C is not set) and a FeCo-5m / NC-800 catalyst prepared by two-step heating (see Example 1) in Friedel-Crafts acylation reaction.
[0057] Wherein, the preparation method of FeCo-5m / NC is as follows:
[0058] (1) 1.5 mmol CoSO4·7H2O and 0.8 g polyvinylpyrrolidone (PVP) were dissolved in 80 mL water, and 80 mL of aqueous solution containing 1.0 mmol K3[Fe(CN)6] was added under continuous stirring, and the mixture was stirred and aged for 24 h. The precipitate generated in the reaction was then centrifuged, washed with water, and dried at 80°C to obtain a brick-red solid powder, which was the iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2 (denoted as PBA-FeCo).
[0059] (2) melamine (denoted as m) and the iron-cobalt-based Prussian blue analog (PBA-FeCo) obtained in step (1) are uniformly mixed in a mass ratio of 5:1, and ground to obtain a pyrolysis precursor, denoted as PBA-FeCo / 5m;
[0060] (3) The pyrolysis precursor PBA-FeCo / 5m obtained in step (2) is directly heated to 800°C at a heating rate of 3°C / min in an inert atmosphere and maintained for 3 h. The obtained product is naturally cooled to room temperature, taken out and ground to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst, which is recorded as FeCo-5m / NC.
[0061] like Figure 2 As shown, compared with the catalyst FeCo-5m / NC obtained by direct heating to 800°C, the iron-cobalt bimetallic nanoparticles in the FeCo-5m / NC-800 catalyst obtained by step-by-step pyrolysis are smaller in size and more evenly dispersed in the carbon matrix.
[0062] like Figure 3As shown in the figure, under the condition of adding the same proportion of melamine to the iron-cobalt-based Prussian blue analog (PBA-FeCo) (X=5), the FeCo-5m / NC-800 catalyst prepared by step-by-step pyrolysis has more excellent stability. After multiple cycles, the activity of the catalyst remains at about 90%. However, the stability of the catalyst FeCo-5m / NC obtained by direct one-step pyrolysis is relatively poor. As the cyclic experiment proceeds, its catalytic activity shows a downward trend, indicating that some active metal species have been lost. It is speculated that the main reason is that during the direct one-step temperature increase pyrolysis process, the metal organic framework structure of PBA-FeCo will collapse or shrink sharply, resulting in a large amount of carbon and nitrogen substances being released in the form of gas, causing the iron-cobalt bimetallic nanoparticles to aggregate severely and form larger particles with uneven particle size distribution (such as Figure 2 ), and some of the iron-cobalt bimetallic particles are not completely coated by the graphite carbon layer. On the other hand, when a step-by-step pyrolysis reaction is used, the PBA-FeCo precursor can fully interact with the partially decomposed melamine at a pyrolysis temperature of 550°C, and form iron-cobalt alloy nanoparticles coated with a graphite carbon layer with a more uniform particle size during the subsequent heating process, which makes the obtained FeCo-5m / NC-800 catalyst show higher stability.
[0063] Example 3 Carbon-coated iron-cobalt bimetallic nanoparticle catalyst FeCo-5m / NC-T (T is pyrolysis temperature, T=600, 700 and 800°C) prepared at different pyrolysis reaction temperatures and its application in Friedel-Crafts acylation reaction.
[0064] Taking the synthesis of FeCo-5m / NC-600 catalyst as an example, the specific preparation method is as follows:
[0065] (1) 1.5 mmol CoSO4·7H2O and 0.8 g polyvinylpyrrolidone (PVP) were dissolved in 80 mL water, and 80 mL of aqueous solution containing 1.0 mmol K3[Fe(CN)6] was added under continuous stirring, and the mixture was stirred and aged for 24 h. The precipitate generated in the reaction was then centrifuged, washed with water, and dried at 80°C to obtain a brick-red solid powder, which was the iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2 (denoted as PBA-FeCo).
[0066] (2) melamine (denoted as m) and the iron-cobalt-based Prussian blue analog (PBA-FeCo) obtained in step (1) are uniformly mixed in a mass ratio of 5:1, and ground to obtain a pyrolysis precursor, denoted as PBA-FeCo / 5m;
[0067] (3) The pyrolysis precursor PBA-FeCo / 5m obtained in step (2) is subjected to a programmed temperature pyrolysis reaction in an inert atmosphere, wherein the programmed temperature pyrolysis program is: heating to 550°C at a heating rate of 3°C / min, maintaining for 2 hours, and then heating to the pyrolysis reaction temperature of 600°C at a heating rate of 3°C / min, maintaining for 3 hours; the obtained product is naturally cooled to room temperature, taken out and ground to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst, recorded as FeCo-5m / NC-600.
[0068] In addition, the same precursor PBA-FeCo / 5m was obtained according to the above steps (1), (2) and (3), and the pyrolysis reaction temperature was adjusted. The temperature was first increased to 550°C at the same heating rate and maintained for 2 h, and then increased to 700 and 800°C (see Example 1) respectively, and maintained for 3 h to obtain catalysts FeCo-5m / NC-700 and FeCo-5m / NC-800.
[0069] like Figure 4 As shown in the figure, with the increase of pyrolysis reaction temperature, the diffraction peak attributed to the FeCo alloy phase (PDF#49-1567) gradually strengthens; in addition, the diffraction peak at the peak position of 26° attributed to the (002) crystal plane of the graphite phase becomes more and more obvious. This is due to the synergistic effect of metal ions and nitrogen-containing carbon carriers during the high-temperature pyrolysis process. At the same time, the metal ions are reduced to zero-valent metal alloys and catalyze the formation of surrounding graphite carbon.
[0070] like Figure 5 As shown in the figure, it can be seen that when the pyrolysis reaction temperature is 550 (intermediate temperature of step-by-step pyrolysis) and 600 °C, the morphology obtained is roughly consistent with the precursor PBA-FeCo, both are spherical, and a large amount of flocculent material is attached to its surface. This is because the introduced melamine first decomposes into sheets of g-C3N4 on the surface of PBA-FeCo; then, as the pyrolysis reaction temperature increases, g-C3N4 completely decomposes, a part of it is released in the form of CNx gas, and the other part forms a graphite layer on the metal surface ( Figure 6 ).
[0071] like Figure 7 As shown in the figure, the catalysts prepared at different pyrolysis reaction temperatures all showed high catalytic activity in the Friedel-Crafts acylation reaction of m-xylene and benzoyl chloride. However, the catalysts FeCo-5m / NC-600 and FeCo-5m / NC-700 suffered from the loss of active species during the cyclic reaction and could not be effectively utilized multiple times.
[0072] Example 4 Taking the carbon-coated iron-cobalt bimetallic nanoparticle catalyst FeCo-5m / NC-800 prepared with melamine-modified PBA-FeCo as a precursor as an example, the catalytic effect of the Friedel-Crafts acylation reaction with different aromatic substrates and acylating agents was investigated.
[0073] The preparation process of catalyst FeCo-5m / NC-800 is the same as that in Example 1. The reaction conditions of the Friedel-Crafts acylation reaction are as follows: the molar ratio of different aromatic substrates to the acylating agent is 2:1, the reaction temperature is 130°C, the catalyst dosage is 50 mg, and the reaction results are shown in Table 2.
[0074] Table 2 Friedel-Crafts acylation results of different aromatic substrates and acylating agents
[0075]
[0076] It can be seen from Table 2 that the catalyst FeCo-5m / NC-800 exhibits good catalytic performance in the Friedel-Crafts acylation reaction of different aromatic substrates and acylating agents, and different substituents on the aromatics have different effects on the conversion of acyl chlorides.
[0077] The above is only a preferred specific embodiment of the present invention. The above examples are for illustrating the detailed synthesis of the catalyst of the present invention and its application in Friedel-Crafts acylation reaction, but the protection scope of the present invention is not limited thereto. The selection of the catalyst raw materials, the ratio of each component and the preparation method of the present invention are all within the scope of protection and disclosure of the present invention. Any technician familiar with the technical field within the technical scope disclosed by the present invention, according to the technical solution and the inventive concept of the present invention, shall be equivalently replaced or changed, and all shall be covered within the protection scope of the present invention.
Claims
1. A carbon-coated iron-cobalt bimetallic nanoparticle catalyst, characterized in that: The catalyst is prepared by pyrolysis of a mixture of an iron-cobalt-based Prussian blue analog and melamine, and comprises iron-cobalt bimetallic nanoparticles and a graphite carbon layer, wherein the surface of the iron-cobalt bimetallic nanoparticles is coated with a graphite carbon layer, the particle size of the iron-cobalt bimetallic nanoparticles is 10-90 nm, the thickness of the graphite carbon layer is 1-10 nm, the total content of iron and cobalt bimetallic in the catalyst is 30-80 wt%, wherein the molar ratio of iron to cobalt is 2:3, and the specific surface area of the catalyst is 20-60 m 2 / g; Wherein, the preparation method of the catalyst comprises the following steps: (1) Cobalt salt CoSO4·7H2O, polyvinyl pyrrolidone and water are mixed uniformly, K3[Fe(CN)6] is added to the obtained mixed solution and stirred uniformly, and then an aging reaction is carried out at room temperature. The obtained reaction solution is centrifuged, washed with water, and dried to obtain an iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2, which is denoted as PBA-FeCo; wherein the mass ratio of the cobalt salt CoSO4·7H2O to polyvinyl pyrrolidone is 0.3-0.8:1; and the molar ratio of the cobalt salt CoSO4·7H2O to K3[Fe(CN)6] is 1.0-2.0:1; (2) uniformly mixing melamine and the iron-cobalt-based Prussian blue analogue obtained in step (1) to obtain a pyrolysis precursor, denoted as PBA-FeCo / Xm; wherein the mass ratio of melamine to the iron-cobalt-based Prussian blue analogue is 1:1, 5:1 or 10:1; (3) The pyrolysis precursor obtained in step (2) is subjected to a programmed temperature pyrolysis reaction in an inert atmosphere to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst, denoted as FeCo-Xm / NC-T; wherein the programmed temperature pyrolysis procedure is: heating to 550°C at a heating rate of 1-5°C / min, maintaining for 1-3 h, and then heating to 600-1000°C at a heating rate of 1-5°C / min, and maintaining for 1-4 h.
2. The method for preparing the carbon-coated iron-cobalt bimetallic nanoparticle catalyst according to claim 1, characterized in that: It includes the following steps: (1) Cobalt salt CoSO4·7H2O, polyvinyl pyrrolidone and water are mixed uniformly, K3[Fe(CN)6] is added to the obtained mixed solution and stirred uniformly, and then an aging reaction is carried out at room temperature. The obtained reaction solution is centrifuged, washed with water, and dried to obtain an iron-cobalt-based Prussian blue analog Co3[Fe(CN)6]2, which is denoted as PBA-FeCo; wherein the mass ratio of the cobalt salt CoSO4·7H2O to polyvinyl pyrrolidone is 0.3-0.8:1; and the molar ratio of the cobalt salt CoSO4·7H2O to K3[Fe(CN)6] is 1.0-2.0:1; (2) uniformly mixing melamine and the iron-cobalt-based Prussian blue analogue obtained in step (1) to obtain a pyrolysis precursor, denoted as PBA-FeCo / Xm; wherein the mass ratio of melamine to the iron-cobalt-based Prussian blue analogue is 1:1, 5:1 or 10:1; (3) The pyrolysis precursor obtained in step (2) is subjected to a programmed temperature pyrolysis reaction in an inert atmosphere to obtain a carbon-coated iron-cobalt bimetallic nanoparticle catalyst, denoted as FeCo-Xm / NC-T; wherein the programmed temperature pyrolysis procedure is: heating to 550°C at a heating rate of 1-5°C / min, maintaining for 1-3 h, and then heating to 600-1000°C at a heating rate of 1-5°C / min, and maintaining for 1-4 h.
3. The method for preparing the carbon-coated iron-cobalt bimetallic nanoparticle catalyst according to claim 2, characterized in that: In step (1), the mass ratio of the cobalt salt CoSO4·7H2O to polyvinyl pyrrolidone is 0.5:1; the molar ratio of the cobalt salt CoSO4·7H2O to K3[Fe(CN)6] is 1.5:
1.
4. The method for preparing the carbon-coated iron-cobalt bimetallic nanoparticle catalyst according to claim 2, characterized in that: In step (1), the aging reaction time is 20 to 30 hours; and the drying temperature is 70 to 90°C.
5. The method for preparing the carbon-coated iron-cobalt bimetallic nanoparticle catalyst according to claim 4, characterized in that: In step (1), the aging reaction time is 24 hours and the drying temperature is 80°C.
6. The method for preparing the carbon-coated iron-cobalt bimetallic nanoparticle catalyst according to claim 2, characterized in that: In step (2), the mass ratio of melamine to the iron-cobalt-based Prussian blue analogue is 5:
1.
7. The method for preparing the carbon-coated iron-cobalt bimetallic nanoparticle catalyst according to claim 2, characterized in that: In step (3), the programmed temperature pyrolysis program is: heating to 550 °C at a heating rate of 3 °C / min, maintaining for 2 h, and then heating to 600-800 °C at a heating rate of 3 °C / min, maintaining for 3 h.
8. Use of the carbon-coated iron-cobalt bimetallic nanoparticle catalyst according to claim 1 as a catalyst.
9. The use according to claim 8, characterized in that: Application as a catalyst in Friedel-Crafts acylation reactions using aromatic hydrocarbons as substrates and acyl chlorides as acylating agents.
10. The use according to claim 9, characterized in that: In the Friedel-Crafts acylation reaction, the molar ratio of the aromatic hydrocarbon to the acyl chloride is 1-5:1; the mass molar ratio of the catalyst to the acyl chloride is 40-100 mg / mol; the reaction temperature is 90-150° C.; the reaction time is 1-8 hours; the aromatic hydrocarbon is one or more of toluene, o-xylene, m-xylene, p-xylene, mesitylene, toluene or o-phenylenedimethyl ether; and the acyl chloride is one or more of benzoyl chloride, p-methylbenzoyl chloride or p-fluorobenzoyl chloride.
11. The use according to claim 10, characterized in that: In the Friedel-Crafts acylation reaction, the molar ratio of the aromatic hydrocarbon to the acyl chloride is 2:1; the mass molar ratio of the catalyst to the acyl chloride is 50 mg / mol; the reaction temperature is 130° C.; the aromatic hydrocarbon is m-xylene, mesitylene or o-phenylenedimethyl ether; and the acyl chloride is benzoyl chloride.
Citation Information
Patent Citations
Nitrogen-doped graphite carbon-coated iron nanoparticle catalysts, preparation methods and their applications in Friedel-Crafts acylation reactions
CN109772406B
N and S dual-doped carbon nanotube-coated FexC catalyst and preparation method and application thereof
CN105826572A
Preparation method and application of 4,4'-dihalide acetodiphenyl
CN105985227A
Method for synthesizing alkyl aromatic ketone by catalytically oxidating alkyl aromatic hydrocarbon and preparation method for catalyst
CN109053398A
Preparation method of nanometer material with carbon-coated metal particle anchoring structure