Composite flooding system and preparation method thereof and method for deep flooding of oil field

By using acrylamide multi-component copolymers and silica nanoparticle composites with alkyl-modified surfaces in medium and high permeability reservoirs, the problem of insufficient viscosity and stability of the existing control and flooding system in deep reservoirs is solved. , achieving efficient deep control and flooding effects and improving oilfield production efficiency.

CN116064008BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111284739.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-01
Publication Date
2024-10-15
Estimated Expiration
2041-11-01

AI Technical Summary

Technical Problem

The existing control and flooding system has insufficient viscosity-increasing effect of the injection phase in medium and high permeability reservoirs, and has low aging and shear viscosity retention rates. It cannot meet the differentiated control needs of different levels of water flooding zones, and it is difficult to realize deep control and flooding of ores. Field effects make it difficult to profitably develop oil fields.

Method used

It uses acrylamide multi-copolymer and silica nanoparticles whose surface is modified by alkyl groups to form a composite with high temperature resistance and salt resistance, water phase viscosity enhancement and high aging shear viscosity retention rate through hydrophobic association interaction. The composite control and flooding system is suitable for deep control and flooding of medium and high permeability oil reservoirs.

Benefits of technology

It achieves the stability and high efficiency of the composite control and flooding system, which is suitable for industrial production applications. It can effectively increase viscosity and oil displacement in deep reservoirs, improve the sweep efficiency of injected water, and meet the needs of improving the quality and efficiency of mature oil fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003332584840000031
    Figure BDA0003332584840000031
  • Figure BDA0003332584840000041
    Figure BDA0003332584840000041
  • Figure BDA0003332584840000081
    Figure BDA0003332584840000081
Patent Text Reader

Abstract

The present invention relates to the field of oil displacement agents, and discloses a composite displacement system and a preparation method thereof, as well as a method for deep displacement of oil fields. The composite provided by the present invention contains an acrylamide multi-polymer and silicon dioxide nanoparticles with alkyl modified surfaces, and has good stability, water solubility, water phase viscosity increase and viscosity retention rate, thereby playing multiple functions of strong thickening, high temperature and high shear viscosity retention, and is particularly suitable for deep displacement of medium and high permeability reservoirs, and has great application significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of oil displacement agents, and in particular to a composite displacement control system and a preparation method thereof, and a method for deep displacement control in an oil field. Background Art

[0002] At present, the old oil fields in eastern my country have generally entered the "two special and one high" development stage of extremely high water content, extremely high recoverable reserves and high cost development. Combined with the current low oil price situation and the complex reservoir heterogeneity conditions of old oil fields, the previous high-efficiency recovery technology faces severe challenges, making the efficient development of oil fields more and more difficult. For example, the well network of the middle layer of old oil fields has been generally adjusted, and there is not much room for large-scale adjustment under the low oil price situation. For another example, the low-cost stratified water injection technology has great difficulty in regulating the contradictions within the layer and on the plane, and cannot meet the needs of improving the recovery rate and improving economic efficiency in the "two special and one high" development stage of old oil fields.

[0003] Deep flooding technology has the characteristics of deep migration and controllable plugging, and is currently one of the most important methods for improving the heterogeneity of medium and high permeability oil reservoirs. However, the existing flooding system has insufficient viscosity-enhancing effect on the injected phase, and the retention rate of aging and shear viscosity is low during the migration to the deep reservoir, which cannot meet the differentiated regulation needs of different levels of water drive zones and it is difficult to achieve the overall deep flooding effect. Therefore, it is urgent to design and develop a new composite and efficient flooding system based on the characteristics of the current medium and high permeability oil reservoirs, so as to meet the needs of plugging, increasing resistance and oil displacement in medium and high permeability oil reservoirs, realize the deep liquid flow diversion in the water consumption zone, and improve the swept efficiency of the injected water, so as to achieve the effect of improving the quality and efficiency of old oilfield exploitation. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a composite displacement system and a preparation method thereof as well as a method for deep displacement of an oil field. The composite displacement system (composite displacement agent) has both profile control and oil displacement functions and can meet the needs of deep displacement of medium and high permeability oil reservoirs, and has good viscosity increasing effect and high aging and shear viscosity retention rate.

[0005] In order to achieve the above object, the present invention provides a composite with a flooding function, which contains an acrylamide multipolymer and silicon dioxide nanoparticles with alkyl modified surfaces.

[0006] A second aspect of the present invention provides a composite flooding system, which comprises the composite as described above and a second solvent.

[0007] A third aspect of the present invention provides a method for preparing a composite profile control and displacement system, the method comprising:

[0008] In the presence of a second solvent, the silicon dioxide nanoparticles whose surfaces are modified by alkyl groups are mixed with the acrylamide multi-polymer to obtain a composite control and displacement system.

[0009] A fourth aspect of the present invention provides a method for deep oilfield flooding, the method comprising applying a flooding agent to oil wells in an oilfield well group, wherein the flooding agent is the composite flooding system as described above or a composite flooding system prepared by the method as described above.

[0010] Through the above technical solution, the present invention can achieve the following beneficial effects:

[0011] (1) The composite flooding system provided by the present invention has good temperature resistance and salt resistance, and can meet the needs of deep flooding in medium and high permeability oil reservoirs;

[0012] (2) The composite flooding system provided by the present invention has good water solubility, good water phase viscosity increasing effect and filterability, and high aging and shear viscosity retention rates, good stability, and is suitable for industrial production applications;

[0013] (3) The preparation method of the composite flooding system provided by the present invention is simple, the raw materials are easily available, and it is suitable for large-scale production and application.

[0014] (4) The composite flooding system provided by the present invention can be mixed with a solvent (water) and an active component (multipolymer and nanoparticles, i.e., the composite with flooding function provided by the present invention) before use. That is, the composite can be first transported to a mining site where it is needed, and then prepared into a composite flooding system on site for use, so that the composite flooding system provided by the present invention is more convenient to transport, store and use. DETAILED DESCRIPTION

[0015] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0016] In the present invention, the "first" and "second" in "first solvent", "second solvent", "first mixture" and "second mixture" are only used to facilitate the distinction between solvents and mixing operations in different steps in the description.

[0017] The inventors of the present invention cleverly discovered during the research process that a mixture obtained by compounding certain acrylamide multi-polymers with nanoparticles with alkyl modified surfaces (such as silica nanoparticles with alkyl modified surfaces) has good flooding and adjustment functions, especially good temperature and salt resistance, water phase viscosity increasing properties, and high aging and shear viscosity retention rates, and is very suitable for deep flooding and adjustment.

[0018] In one aspect, the present invention provides a composite having a flooding function, wherein the composite comprises an acrylamide multipolymer and silicon dioxide nanoparticles with surfaces modified by alkyl groups. The acrylamide multipolymer and the silicon dioxide nanoparticles with surfaces modified by alkyl groups interact with each other through hydrophobic association.

[0019] According to a preferred embodiment of the present invention, the acrylamide multipolymer contains a first structural unit R provided by acrylamide. 1 , the second structural unit R provided by the substance represented by formula I 2 The third structural unit R is provided by the substance represented by formula II 3 .

[0020]

[0021] In Formula I, M 1 It is H, K or Na.

[0022] In formula II, X is O or NH, preferably NH; R is selected from C 1-18 Alkyl and / or phenyl, preferably C 6-16 Alkyl and / or phenyl.

[0023] In order to further improve the viscosity-increasing effect of the composite, preferably, in Formula II, R is selected from C 6-16 alkyl.

[0024] According to a preferred embodiment of the present invention, the first structural unit R 1 The invention comprises a structural unit represented by formula III and a structural unit represented by formula IV. Specifically, after the monomer mixture is polymerized, the acrylamide multi-polymer obtained by polymerization is contacted with an inorganic alkaline compound under conventional hydrolysis conditions well known to those skilled in the art, and the hydrolysis conditions allow the acrylamide structural unit in the copolymer to be partially hydrolyzed into a structural unit having formula IV.

[0025]

[0026] Among them, M 2 Na or K is preferred.

[0027] According to a preferred embodiment of the present invention, based on 100 parts by weight of the acrylamide multipolymer, the first structural unit R1 The content of the second structural unit R is 80-96 parts by weight. 2 The content of the third structural unit R is 2-10 parts by weight. 3 The content is 2-10 parts by weight.

[0028] Preferably, in the acrylamide multipolymer, the second structural unit R 2 With the third structural unit R 3 The weight ratio is 1:4-4:1.

[0029] According to a preferred embodiment of the present invention, the viscosity average molecular weight of the acrylamide multi-polymer is 10 million to 20 million, more preferably 10 million to 15 million. Specifically, the multi-polymer is preferably a random copolymer.

[0030] According to a preferred embodiment of the present invention, in the nanoparticles whose surfaces are modified with alkyl groups, the molar ratio of silicon dioxide to alkyl groups is 1:0.3-0.8.

[0031] According to a preferred embodiment of the present invention, in the nanoparticles whose surfaces are modified with alkyl groups, the substance providing the alkyl groups is alkyltrialkoxysilane.

[0032] Preferably, the substance providing the alkyl group is alkyltriethoxysilane and / or alkyltrimethoxysilane. 1-18 The normal alkyl group is preferably C 6-14 For example, C 1-18 The normal alkyl group may be methyl, ethyl, n-propyl, n-butyl, isobutyl, n-hexyl, n-octyl or even n-octadecyl.

[0033] According to a preferred embodiment of the present invention, the number average particle size of the silica nanoparticles whose surfaces are modified with alkyl groups is 20-200 nm.

[0034] According to a preferred embodiment of the present invention, the silicon dioxide nanoparticles with alkyl modified surfaces are prepared by the following method:

[0035] In a first solvent, the silica nanoparticles are first mixed with an alkyl modifier, and then solid-liquid separation is performed to obtain silica nanoparticles with surfaces modified by alkyl groups. The alkyl modifier is connected to the silica nanoparticles via a covalent bond.

[0036] Preferably, the number average particle size of the silicon dioxide nanoparticles is 20-90 nm.

[0037] Preferably, the first mixing is performed under the condition of a first stirring, and the rotation speed of the first stirring is 250-720 rpm.

[0038] Preferably, the temperature of the first mixing is 20-80° C. and the time is 10-14 h.

[0039] Preferably, based on 1 g of the silica nanoparticles, the amount of the first solvent used is 70-100 mL.

[0040] Preferably, the first solvent is an organic solvent, preferably at least one of cyclohexane, n-hexane and petroleum ether.

[0041] Preferably, based on 1 g of the nano-silica particles, the amount of the alkyl modifier is preferably 1-10 g, more preferably 1.8-6 g.

[0042] Preferably, the alkyl modifier is an alkyltrialkoxysilane.

[0043] More preferably, the alkyl modifier is alkyltriethoxysilane and / or alkyltrimethoxysilane. 1-18 The normal alkyl group is preferably C 6-14 of normal alkyl.

[0044] In the present invention, in order to accelerate the dispersion of nano-silicon dioxide particles, the nano-silicon dioxide particles can be dispersed in a first solvent such as an organic solvent such as cyclohexane under ultrasonic conditions, and the frequency of the ultrasonic wave is preferably 20-40 kHz.

[0045] In the present invention, the solid-liquid separation method is not limited, and any solid-liquid separation method currently available in the art can be used for the separation. For example, the solid-liquid separation can be achieved by centrifugation.

[0046] Preferably, the centrifugal rotation speed is 2000-3000 rpm, and the time is 20-50 minutes.

[0047] In the present invention, the method further comprises: washing and drying the solid obtained after the solid-liquid separation, wherein the washing liquid used for washing is preferably at least one of ethanol, methanol and acetone, and the washing is preferably performed 2-5 times.

[0048] In the present invention, the drying may be carried out by conventional methods in the art. Preferably, the drying is carried out in a drying device. The drying conditions may include a drying temperature of 60-80° C. and a drying time of 22-26 hours.

[0049] In the present invention, the first mixing is preferably carried out under weak alkaline conditions, preferably under conditions of pH 7 to 9. Specifically, the pH value of the first mixed system can be adjusted to 7 to 9 by methods known to those skilled in the art, for example, ammonia water can be added to the first mixed system to adjust the pH value of the first mixed system to 7 to 9.

[0050] According to a preferred embodiment of the present invention, in the composite, the weight ratio of the silica nanoparticles with alkyl groups modified on the surface to the acrylamide multi-polymer is 1:5-20, preferably 1:10-15.

[0051] The second aspect of the present invention provides a composite flooding system, which comprises the composite material and the second solvent as described above. The composite flooding system has good flooding function and is particularly suitable for deep flooding.

[0052] Preferably, the concentration of the composite in the composite flooding system is 1200-5000 ppm. That is, the total concentration of the silica nanoparticles with alkyl groups modified on the surface and the acrylamide multi-polymer is 1200-5000 ppm.

[0053] Preferably, the second solvent is water. The "water" may be pure water (e.g., tap water, distilled water, deionized water, etc.), or an aqueous solution. For example, it may be an aqueous solution of salt. For ease of use on site, water with a certain degree of mineralization (e.g., on-site water such as Victory II type salt water) may be used as the second solvent.

[0054] More preferably, the second solvent is water with a mineralization of 10000-20000 mg / L and a calcium and magnesium ion content of 300-800 mg / L at a temperature of 65-85°C. "Mineralization" refers to the total mass of various salts in 1L of salt water, which can be measured by ion chromatography. "Calcium and magnesium ion content" refers to the total mass of Ca in 1L of the salt water. 2+ and Mg 2+ The mass content can be determined by chemical measurement according to the formula during preparation, or by ion chromatography.

[0055] The third aspect of the present invention provides a method for preparing a composite profile control and displacement system (as described above), the method comprising:

[0056] In the presence of a second solvent, the silicon dioxide nanoparticles whose surfaces are modified by alkyl groups are mixed with the acrylamide multi-polymer to obtain a composite control and displacement system.

[0057] According to a preferred embodiment of the present invention, the surface of the silica nanoparticles modified by alkyl is dispersed in the second solvent, and after emulsification and ultrasound, a mixed solution A containing the surface of the silica nanoparticles modified by alkyl is obtained. The acrylamide multipolymer is dissolved in the mixed solution A under stirring conditions, and is allowed to stand to obtain a composite flooding system (for deep flooding). Specifically, the second solvent is preferably water. Considering the field conditions of the reservoir, field water with a salinity of 10000-20000 mg / L and a calcium and magnesium ion content of 300-800 mg / L (for example, Victory II type brine that meets the above conditions) is selected as the second solvent. The emulsification time is 10-20 minutes. The frequency of the ultrasound is 25-40kHz, and the time is 0.5-1.5h. When dissolving the acrylamide multipolymer, it is carried out under stirring conditions. Preferably, the acrylamide multipolymer is contacted with the mixed solution A within 25-40s under stirring conditions of 200-300 rpm. Then, the mixture is stirred for 1.5-3 hours at a temperature of 20-40° C. and 500-700 rpm. The mixture is stirred for a period of time to obtain the composite flooding system (for deep flooding). Preferably, the stirring time is 6-12 hours at a temperature of 20-40° C., and the pH value does not need to be specially adjusted during the process.

[0058] According to a preferred embodiment of the present invention, the method further comprises the step of preparing an acrylamide multi-polymer by polymerizing the monomer mixture in water under free radical aqueous solution polymerization conditions in the presence of an initiator.

[0059] Preferably, the monomer mixture contains acrylamide, a substance represented by formula I and a substance represented by formula II.

[0060]

[0061] Among them, in formula I, M 1 It is H, K or Na.

[0062] In formula II, X is O or NH, preferably NH. R is selected from C 1-18 Alkyl and / or phenyl, preferably C 6-16 Alkyl and / or phenyl, more preferably C 6-16 alkyl.

[0063] According to a preferred embodiment of the present invention, based on 100 parts by weight of the monomer mixture, the content of acrylamide is 80-96 parts by weight, the content of the substance represented by formula I is 2-10 parts by weight, and the content of the substance represented by formula II is 2-10 parts by weight.

[0064] According to a preferred embodiment of the present invention, the initiator is selected from azo initiators and / or redox initiators, and more preferably redox initiators.

[0065] Preferably, the redox initiator is selected from at least one of sulfate and sulfite redox initiators, persulfate and thiourea redox initiators, persulfate and organic salt redox initiators, persulfate and sulfite redox initiators, and ammonium persulfate and fatty amine redox initiators.

[0066] More preferably, the sulfate is selected from at least one of sodium sulfate, potassium sulfate and ammonium sulfate.

[0067] More preferably, the sulfite is selected from at least one of sodium sulfite, potassium sulfite, sodium bisulfite, potassium bisulfite and ammonium sulfite.

[0068] More preferably, the persulfate is selected from at least one of sodium persulfate, potassium persulfate and ammonium persulfate.

[0069] More preferably, the organic salt is selected from at least one of thiourea, sodium acetate and potassium acetate.

[0070] More preferably, the fatty amine is selected from at least one of ammonium acetate, N,N-tetramethylethylenediamine and diethylamine.

[0071] Further preferably, the redox initiator is selected from at least one of sodium sulfate and sodium sulfite, potassium sulfate and potassium sulfite, ammonium sulfate and sodium bisulfite, ammonium sulfate and ammonium sulfite, sodium persulfate and thiourea, potassium persulfate and thiourea, ammonium persulfate and thiourea, sodium persulfate and potassium acetate, potassium persulfate and potassium acetate, ammonium persulfate and ammonium acetate, ammonium persulfate and N,N-tetramethylethylenediamine, and ammonium persulfate and diethylamine.

[0072] In the present invention, there is no particular limitation on the amount of the initiator. According to a preferred embodiment of the present invention, based on 50 g of the monomer mixture, the amount of the initiator is 0.0022-0.0035 g.

[0073] According to a preferred embodiment of the present invention, the polymerization reaction is carried out in the presence of a complexing agent and urea.

[0074] Preferably, the complexing agent is selected from at least one of disodium ethylenediaminetetraacetate, sodium nitrilotriacetate and diethylenetriamine pentacarboxylate, preferably disodium ethylenediaminetetraacetate.

[0075] Preferably, the amount of urea used is 0.01-0.1 wt % based on the total weight of the monomer mixture.

[0076] Preferably, the weight ratio of the urea to the complexing agent is 1-10:1. Specifically, the complexing agent and urea are used to complex metal ions, improve the conversion rate of the polymerized monomers and play a solubilizing role. Usually, the complexing agent and urea are used in the form of their aqueous solutions, wherein the complexing agent aqueous solution is preferably 1-3% by weight of the complexing agent aqueous solution, and the urea aqueous solution is preferably 1-3% by weight of the urea aqueous solution.

[0077] According to a preferred embodiment of the present invention, the conditions of the polymerization reaction include: temperature of -10°C to 80°C, time of 2-30 hours, and pH value of 5-10.

[0078] Preferably, the polymerization reaction conditions include: temperature of 5-60° C., time of 8-20 hours, and pH of 6-10.

[0079] According to a preferred embodiment of the present invention, the method further comprises the step of preparing the silica nanoparticles whose surfaces are modified by alkyl groups:

[0080] In a first solvent, the nano-silica particles are first mixed with an alkyl modifier, and then solid-liquid separation is performed to obtain silica nano-particles with surfaces modified by alkyl groups.

[0081] Preferably, the first mixing is performed under the condition of a first stirring, and the rotation speed of the first stirring is 250-720 rpm.

[0082] Preferably, the temperature of the first mixing is 20-80° C. and the time is 10-14 h.

[0083] In the present invention, the amount of the alkyl modifier is such that the molar ratio of silicon dioxide to alkyl in the obtained nanoparticles whose surfaces are modified by alkyl is 1:0.3-0.8. In the present invention, it is believed that the etherification reaction between the alkyl modifier and the nanoparticles is a complete reaction, so the molar ratio can be obtained by estimating the feed ratio. Preferably, based on 1g of the nano-silica particles, the amount of the alkyl modifier is 1-10g, more preferably 1.2-5g. As mentioned above, the number average particle size of the silicon dioxide nanoparticles is preferably 20-200nm.

[0084] Preferably, based on 1 g of the nano-silicon dioxide particles, the amount of the first solvent used is 70-100 mL.

[0085] Preferably, the first solvent is an organic solvent, preferably at least one of cyclohexane, n-hexane and petroleum ether.

[0086] Preferably, the alkyl modifier is an alkyltrialkoxysilane.

[0087] More preferably, the alkyl modifier is alkyltriethoxysilane and / or alkyltrimethoxysilane. 1-18 The normal alkyl group is preferably C 6-14 of normal alkyl.

[0088] According to a preferred embodiment of the present invention, the amounts of the silica nanoparticles with alkyl groups modified on the surface and the acrylamide multipolymer are such that the weight ratio of the silica nanoparticles with alkyl groups modified on the surface to the acrylamide multipolymer is 1:5-20, preferably 1:10-15.

[0089] Preferably, the amounts of the silicon dioxide nanoparticles with alkyl groups modified on the surface and the acrylamide multipolymer are such that the total concentration of the silicon dioxide nanoparticles with alkyl groups modified on the surface and the acrylamide multipolymer in the composite flooding system is 1200-5000 ppm.

[0090] Preferably, the second solvent is water. The "water" may be pure water (e.g., tap water, distilled water, deionized water, etc.), or an aqueous solution. For example, it may be an aqueous solution of salt. For ease of use on site, water with a certain degree of mineralization (e.g., on-site water such as Victory II type salt water) may be used as the second solvent.

[0091] More preferably, considering the reservoir site conditions, water with a salinity of 10000-20000 mg / L and a calcium and magnesium ion content of 300-800 mg / L is selected as the second solvent.

[0092] According to a preferred embodiment of the present invention, the polymerization reaction is carried out in the presence of a complexing agent and urea, and the mode and conditions of the polymerization reaction are as follows: the monomer mixture is dissolved in a solvent, and the pH value of the obtained monomer mixture solution is adjusted to 6-10, then the complexing agent and urea are added, and then nitrogen is passed into the reaction system at 5-15°C for 10-30 minutes, and then an initiator is added, and then nitrogen is passed for 5-30 minutes until the reaction solution begins to become viscous, and then the nitrogen is stopped and adiabatic polymerization is carried out for 4-10 hours. After the polymerization reaction is completed, the rubber is sheared, granulated, hydrolyzed, dried and powdered to obtain an acrylamide multipolymer.

[0093] The inventors of the present invention unexpectedly discovered that the polymer obtained by adopting the above-mentioned polymerization reaction mode and polymerization reaction conditions has more excellent properties. Specifically, in order to overcome oxygen inhibition and obtain a polymer with a larger molecular weight, preferably, the polymerization reaction is carried out in an inert atmosphere. Among them, the inert gas used to maintain the inert atmosphere can be various existing gases or gas mixtures that do not react with raw materials and products, for example, it can be nitrogen or at least one of the gases of the zeroth group elements in the periodic table. From the perspective of economy, the inert atmosphere is preferably provided by nitrogen. In the present invention, hydrolysis refers to the use of a stoichiometric (related to the degree of hydrolysis) concentration of 35-40% by weight NaOH solution, which is evenly sprayed on acrylamide polymer particles with a particle size of 2-4mm, and after being evenly dispersed, placed in a water bath at a temperature of 60-90°C and heated for 2-8h. The hydrolysis step is a conventional step for preparing acrylamide polymers and will not be repeated here.

[0094] In the present invention, the content of each structural unit in the copolymer can be tested by conventional methods in the prior art, such as infrared spectroscopy, nuclear magnetic resonance, and the amount of monomers added during the polymerization process.

[0095] In the present invention, the content of each structural unit in the polymer is determined by the monomer feed amount. Specifically, the feed ratio of each monomer actually participating in the polymerization is determined by testing the content of unreacted monomers, and then the content of each structural unit in the polymer is determined.

[0096] Furthermore, in the present invention, the content of each unreacted (residual) monomer in the polymerization product is less than 0.02 wt%, indicating that all monomers are substantially involved in the polymerization reaction. Specifically, the content of the residual monomer is determined by liquid chromatography.

[0097] The composite flooding system prepared by the method described above also belongs to the content of the present invention.

[0098] A fourth aspect of the present invention provides a method for deep oilfield flooding, the method comprising applying a flooding agent to an oil well in an oilfield well group, wherein the flooding agent is the composite flooding system as described above or the composite flooding system prepared by the method as described above. The composite flooding system of the present invention can meet the needs of deep flooding of medium and high permeability oil reservoirs.

[0099] The present invention will be described in detail below by way of examples. It should be understood that the following examples are only used to further explain and illustrate the content of the present invention by way of example, and are not intended to limit the present invention.

[0100] In the following examples, the reagents used are all commercially available analytical reagents. Room temperature refers to 25°C. Degree of hydrolysis refers to molar percentage. Nano silicon dioxide particles are purchased from Shanghai McLean Biochemical Technology Co., Ltd., with a particle size of 20-90nm. The preparation water (i.e., the second solvent in the foregoing content) is a victory II type salt water with a mineralization of about 19334mg / L and a calcium and magnesium ion content of about 514mg / L. Partially hydrolyzed polyacrylamide is purchased from France Aisen Company, with a trade name of 1630s, a degree of hydrolysis of 33%, and a viscosity-average molecular weight of 13 million. Nano iron trioxide magnetic particles are purchased from Inokai Company, with a particle size of 20-80nm. The alkyl triethoxysilanes used in the embodiments are all purchased from Inokai Company, with a purity of> 95% and a density of about 0.996g / mL.

[0101] Preparation Example 1

[0102] This preparation example is used to illustrate the preparation of acrylamide multi-polymer.

[0103] In this preparation example, the hydrolysis step is: add a stoichiometric 40 wt% sodium hydroxide solution (calculated based on a hydrolysis degree of 33%) and spray it evenly on the 2-4 mm diameter particles, mix well and heat in a 70° C. water bath for 6 hours.

[0104] (I) Acrylamide multipolymer P1

[0105] 45g acrylamide, 2.5g 2-acrylamido-2-methylpropanesulfonic acid and 2.5g N-hexyl acrylamide were dissolved in 300g deionized water, and the pH value was adjusted to 7 with sodium hydroxide. Then, 0.8g of disodium ethylenediaminetetraacetate aqueous solution (1 wt%) and 0.8g of urea aqueous solution (1 wt%) were added and mixed evenly. After the mixed solution was cooled to 5°C, it was placed in a container and nitrogen was introduced for 30min, and then 0.8g of ammonium persulfate aqueous solution (1 wt%) and 1.6g of sodium bisulfite aqueous solution (1 wt%) were added, and then nitrogen was introduced for 10 minutes until the reaction solution began to become viscous. Then, nitrogen was stopped and adiabatic polymerization was carried out for 8h. The residual monomer content in the polymerization product was all below 0.02 wt%. After the polymerization reaction, the rubber was cut, granulated, hydrolyzed, dried and powdered to obtain an acrylamide multi-polymer P1, whose viscosity-average molecular weight was about 14.1 million (obtained by referring to GB 17514-2008 standard detection, the same below).

[0106] (ii) Acrylamide multipolymer P2

[0107] 45g acrylamide, 2.5g 2-acrylamido-2-methylpropanesulfonic acid and 2.5g N-hexadecyl acrylamide were dissolved in 300g deionized water, and the pH value was adjusted to 10 with sodium hydroxide. Then, 0.3g of disodium ethylenediaminetetraacetate aqueous solution (3 wt%) and 0.3g of urea aqueous solution (3 wt%) were added and mixed evenly. After the mixed solution was cooled to 15°C, it was placed in a container and nitrogen was introduced for 10 minutes, and then 1.8g of sodium persulfate aqueous solution (1 wt%) and 1.7g of thiourea aqueous solution (1 wt%) were added, and then nitrogen was introduced for 30 minutes until the reaction solution began to become viscous. Then, nitrogen blowing was stopped and adiabatic polymerization was carried out for 10 hours. The residual monomer content in the polymerization product was all below 0.02 wt%. After the polymerization reaction was completed, the rubber was sheared, granulated, hydrolyzed, dried and powdered to obtain acrylamide multipolymer P2, whose viscosity-average molecular weight was about 12.1 million.

[0108] (III) Acrylamide multipolymer P3

[0109] 45g acrylamide, 2.5g 2-acrylamido-2-methylpropanesulfonic acid and 2.5g N-phenylacrylamide were dissolved in 300g deionized water, and the pH value was adjusted to 5 with sodium hydroxide. Then, 0.5g aqueous solution of disodium ethylenediaminetetraacetate (1 wt%) and 0.5g aqueous solution of urea (1 wt%) were added and mixed evenly. After the mixed solution was cooled to 10°C, it was placed in a container and nitrogen was introduced for 20 minutes, and then 1.1g aqueous solution of ammonium sulfate (1 wt%) and 1.1g aqueous solution of ammonium sulfite (1 wt%) were added, and then nitrogen was introduced for another 20 minutes until the reaction solution began to become viscous. Then, nitrogen blowing was stopped and adiabatic polymerization was performed for 4h. The residual monomer content in the polymerization product was all below 0.02 wt%. After the polymerization reaction was completed, the rubber was sheared, granulated, hydrolyzed, dried and powdered to obtain acrylamide multipolymer P3, whose viscosity-average molecular weight was about 16.1 million.

[0110] (IV) Acrylamide multipolymer P4

[0111] According to the method for preparing acrylamide multipolymer P1, the difference is that N-hexyl acrylamide is replaced by N-n-butyl acrylamide to obtain acrylamide multipolymer P4, whose viscosity-average molecular weight is about 13.9 million.

[0112] (V) Acrylamide multipolymer P5

[0113] According to the method for preparing acrylamide multipolymer P1, the difference is that N-hexyl acrylamide is replaced by N-octadecyl acrylamide to obtain acrylamide multipolymer P5, whose viscosity-average molecular weight is about 9.95 million.

[0114] (VI) Acrylamide multipolymer P6

[0115] According to the method for preparing acrylamide multipolymer P1, except that 40g of acrylamide, 5g of 2-acrylamido-2-methylpropanesulfonic acid and 5g of N-hexadecyl acrylamide were added, acrylamide multipolymer P6 was obtained, and its viscosity average molecular weight was about 11.9 million.

[0116] (VII) Acrylamide multipolymer P7

[0117] The method for preparing acrylamide multipolymer P1 was followed, except that 47.5 g of acrylamide, 1.25 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.25 g of N-hexadecylacrylamide were added to obtain acrylamide multipolymer P7, whose viscosity-average molecular weight was about 18.2 million.

[0118] (VIII) Acrylamide multipolymer P8

[0119] The method for preparing acrylamide multipolymer P1 was followed, except that 45 g of acrylamide, 1 g of 2-acrylamido-2-methylpropanesulfonic acid and 4 g of N-hexylacrylamide were added to obtain acrylamide multipolymer P6, whose viscosity-average molecular weight was about 14.9 million.

[0120] (IX) Acrylamide multipolymer P9

[0121] The method for preparing acrylamide multipolymer P1 was followed, except that 45 g of acrylamide, 4 g of 2-acrylamido-2-methylpropanesulfonic acid and 1 g of N-hexylacrylamide were added to obtain acrylamide multipolymer P6, whose viscosity-average molecular weight was about 12 million.

[0122] Preparation Example 2

[0123] This preparation example is used to illustrate the preparation of silica nanoparticles whose surfaces are modified with alkyl groups.

[0124] (I) Surface-modified silica nanoparticles N1

[0125] 1 g of nano-silica particles were dispersed in 80 mL of cyclohexane and dispersed stably by ultrasound (40 kHz) for 1 hour. 3.12 mL of octyltriethoxysilane was added and stirred at 25°C for 12 hours (stirring speed 480 rpm). The mixture was centrifuged at 2500 rpm for 30 minutes, and the obtained precipitate was washed 3 times with ethanol and dried in an oven at 70°C for 24 hours to obtain silica nanoparticles N1 with octyl groups modified on the surface.

[0126] (ii) Silica nanoparticles N2 modified with alkyl groups

[0127] 1 g of nano-silica particles were dispersed in 100 mL of cyclohexane and dispersed stably by ultrasound (30 kHz) for 1 hour. 2.09 mL of butyltriethoxysilane was added and stirred at 25°C for 10 hours (stirring speed 250 rpm). The mixture was centrifuged at 2000 rpm for 50 minutes, and the obtained precipitate was washed twice with ethanol and dried in an oven at 60°C for 26 hours to obtain silica nanoparticles N2 with butyl groups modified on the surface.

[0128] (III) Surface-modified silica nanoparticles N3

[0129] 1 g of nano-silica particles were dispersed in 70 mL of cyclohexane and dispersed stably by ultrasound (20 kHz) for 1 hour. 3.65 mL of hexadecyltriethoxysilane was added and stirred at 25° C. for 14 hours (stirring speed 720 rpm). The mixture was centrifuged at 3000 rpm for 20 minutes, and the obtained precipitate was washed with ethanol 5 times and dried in an oven at 80° C. for 22 hours to obtain silica nanoparticles N3 with hexadecyl modified surfaces.

[0130] Example 1

[0131] (1) The surface octyl-modified silica nanoparticles N1 obtained in Preparation Example 2 were weighed, slowly dispersed in the prepared water, rapidly emulsified for 15 min using an emulsifier, and then ultrasonicated for 1 hour (30 kHz) using an ultrasonic cleaner to obtain a nanoparticle dispersion.

[0132] (2) Place the nanoparticle dispersion obtained in step (1) in a beaker, weigh the acrylamide multipolymer P1 obtained in Preparation Example 1, start a constant speed stirrer and slowly add the polymer P1 along the vortex wall at a speed of 300 rpm for 30 seconds, then adjust the stirring rate to 500 rpm, stir for 2 hours, and obtain a mixed suspension of nanoparticles and acrylamide multipolymer. The content of the silicon dioxide nanoparticles N1 with octyl modified on the surface is 150ppm, the content of the acrylamide multipolymer P1 is 1800ppm, and the rest is the prepared aqueous solution. Then continue to stir at 25°C and a speed of 400 rpm for 8 hours to make the nano silicon dioxide particles and the multipolymer in the suspension evenly mixed and fully act.

[0133] (3) The suspension was allowed to stand at 25°C for 24 h. If no obvious precipitation or stratification occurred, a composite flooding system was obtained.

[0134] Example 2

[0135] The composite profile control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P2 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0136] Example 3

[0137] The composite control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P3 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0138] Example 4

[0139] The composite control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P4 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0140] Example 5

[0141] The composite control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P5 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0142] Example 6

[0143] The composite profile control and displacement system was prepared according to the method of Example 1, except that the silicon dioxide nanoparticles N2 with butyl groups modified on the surface obtained in Preparation Example 2 were used instead of the silicon dioxide nanoparticles N1 with octyl groups modified on the surface.

[0144] Example 7

[0145] The composite profile control and displacement system was prepared according to the method of Example 1, except that the silicon dioxide nanoparticles N3 with butyl groups modified on the surface obtained in Preparation Example 2 were used instead of the silicon dioxide nanoparticles N1 with octyl groups modified on the surface.

[0146] Example 8

[0147] The composite control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P6 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0148] Example 9

[0149] The composite control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P7 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0150] Example 10

[0151] The composite flooding system was prepared according to the method of Example 1, except that the amounts of nanoparticles N1 and acrylamide multipolymer P1 were adjusted so that in the composite flooding system, the concentration of silica nanoparticles N1 with octyl groups on the surface was 90 ppm, and the concentration of acrylamide multipolymer P1 was 1800 ppm.

[0152] Embodiment 11

[0153] The composite flooding system was prepared according to the method of Example 1, except that the amounts of nanoparticles N1 and acrylamide multipolymer P1 were adjusted so that in the composite flooding system, the concentration of silica nanoparticles N1 with octyl groups on the surface was 360 ppm, and the concentration of acrylamide multipolymer P1 was 1800 ppm.

[0154] Example 12

[0155] The composite profile control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P8 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0156] Embodiment 13

[0157] The composite control and displacement system was prepared according to the method of Example 1, except that the acrylamide multipolymer P9 obtained in Preparation Example 1 was used instead of the acrylamide multipolymer P1.

[0158] Comparative Example 1

[0159] The composite flooding system was prepared according to the method of Example 1, except that partially hydrolyzed polyacrylamide (trade name: 1630s) was used instead of the acrylamide multipolymer P1.

[0160] Comparative Example 2

[0161] The composite control and displacement system was prepared according to the method of Example 1, except that the silicon dioxide nanoparticles N1 whose surfaces were modified with alkyl groups were replaced with silicon dioxide nanoparticles whose surfaces were not modified.

[0162] Comparative Example 3

[0163] The composite control and displacement system was prepared according to the method of Example 1, except that the silicon dioxide nanoparticles N1 with alkyl modified surfaces were not added.

[0164] Comparative Example 4

[0165] The composite flooding system was prepared according to the method of Example 1, except that the acrylamide multipolymer P1 was not added.

[0166] Comparative Example 5

[0167] The composite control and displacement system was prepared according to the method of Example 1, except that nano-iron oxide magnetic particles were used to replace the silicon dioxide nanoparticles N1 whose surfaces were modified by alkyl groups.

[0168] Test Example 1

[0169] The apparent viscosity of the acrylamide multipolymer obtained in Preparation Example 1 was tested. The specific test method is: at a temperature of 70°C, the acrylamide multipolymer to be tested was added to a Victory II type prepared brine having a salinity of about 20,000 mg / L and a calcium and magnesium ion content of about 300 mg / L to prepare a polymer suspension with a concentration of 1800 ppm, and the apparent viscosity of the suspension was measured by a Brookfield viscometer. The test results are shown in Table 1.

[0170] Test Example 2

[0171] At a temperature of 70° C., the apparent viscosity of the composite profile control system obtained in the above embodiment and comparative example was tested by a Brookfield viscometer. The test results are shown in Table 1.

[0172] Test Example 3

[0173] With reference to Sinopec Enterprise Standard Q / SH3135 438-2017, the aging and shear viscosity retention rates of the composite flooding systems obtained in the above embodiments and comparative examples were tested. The liquid to be tested is the composite flooding system obtained in the above embodiments and comparative examples, and the aging viscosity retention rate is measured after the composite flooding system to be tested is aged in an oven at 70°C for 45 days. The test results are shown in Table 1.

[0174] Test Example 4

[0175] The stability of the composite flooding system obtained in the above examples and comparative examples was tested. The specific detection method is: the composite flooding system to be tested is allowed to stand at room temperature, and the number of days required for clarification is directly observed by visual observation. The more days required for clarification, the better the stability of the system. It should be noted that during the stability test, if the solution still does not become turbid after 45 days, the observation is stopped and the system can be put into use. The test results are shown in Table 1.

[0176] Table 1

[0177]

[0178]

[0179] As can be seen from Table 1, in the control and displacement composite composed of the silicon dioxide nanoparticles and acrylamide multipolymers whose surfaces are modified by alkyl of the present invention, the viscosity of the composite is greatly improved compared with the original polymer through the hydrophobic association synergy of the silicon dioxide nanoparticles and acrylamide multipolymers whose surfaces are modified by alkyl, the stability is good, the aging viscosity retention rate is improved, and the shear viscosity retention rate is stable, which is suitable for deep control and displacement of oil reservoirs. Specifically, after the surface of nano silicon dioxide is hydrophobically modified by alkyl, the hydrophobic association interaction is strengthened with the acrylamide copolymer molecules containing long-chain alkyl hydrophobic groups, so better performance is shown (Example 1 and Comparative Example 2). The acrylamide copolymer with hydrophobic properties also has higher viscosity and viscosity retention rate (Example 1 and Comparative Example 1) with nanoparticles compared with ordinary polyacrylamide. After the nanoparticle-polymer provided by the present invention forms a composite, not only the stability of the nanoparticle is strengthened, but also the interaction between the two is strengthened, and the cross-linking effect of the intermolecular non-bonding action is formed, thereby significantly improving the viscosity of the polymer system (Example 1 and Comparative Examples 3, 4). In addition, in Comparative Example 5, nano-iron trioxide was used to produce precipitation with the polymer, and the stability was too poor to be evaluated. This shows that the composite flooding system prepared under the preferred conditions of the present invention using the acrylamide copolymer and nanoparticles provided by the present invention has good temperature and salt resistance, stability, water solubility, water phase viscosity increase, filterability, aging, and shear viscosity retention rate, thereby having a better flooding effect.

[0180] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A composite material with deep displacement function, characterized in that: The composite contains acrylamide multi-polymer and silicon dioxide nanoparticles with surfaces modified by alkyl groups; The acrylamide multi-polymer contains a first structural unit R1 provided by acrylamide, a second structural unit R2 provided by a substance represented by formula I, and a third structural unit R3 provided by a substance represented by formula II; Formula I Formula II In formula I, M1 is H, K or Na; In formula II, X is NH; R is selected from C 1-18 Alkyl and / or phenyl.

2. The composite according to claim 1, wherein In formula II, R is C 6-16 Alkyl and / or phenyl.

3. The composite according to claim 1, wherein Based on 100 parts by weight of the acrylamide multipolymer, the content of the first structural unit R1 is 80-96 parts by weight, the content of the second structural unit R2 is 2-10 parts by weight, and the content of the third structural unit R3 is 2-10 parts by weight.

4. The composite according to claim 1, wherein The viscosity average molecular weight of the acrylamide multi-polymer is 10 million to 20 million.

5. The composite according to claim 4, wherein The viscosity average molecular weight of the acrylamide multi-polymer is 10 million to 15 million.

6. The composite according to claim 1, wherein In the nanoparticles whose surfaces are modified with alkyl groups, the molar ratio of silicon dioxide to alkyl groups is 1:0.3-0.8; And / or, in the nanoparticles whose surfaces are modified with alkyl groups, the substance providing the alkyl groups is alkyltrialkoxysilane; And / or, the number average particle size of the silica nanoparticles whose surfaces are modified with alkyl groups is 20-200 nm.

7. The composite according to claim 6, wherein In the nanoparticles whose surfaces are modified with alkyl groups, the substance providing the alkyl groups is alkyltriethoxysilane and / or alkyltrimethoxysilane.

8. The composite according to claim 7, wherein Alkyl is C 1-18 of normal alkyl.

9. The composite according to claim 8, wherein Alkyl is C 6-14 of normal alkyl.

10. The composite according to claim 1, wherein The silicon dioxide nanoparticles with alkyl modified surfaces are prepared by the following method: In a first solvent, the silica nanoparticles are first mixed with an alkyl modifier, and then solid-liquid separation is performed to obtain silica nanoparticles with surfaces modified by alkyl groups.

11. The composite according to claim 10, wherein The first mixing is performed under a first stirring condition, and the rotation speed of the first stirring is 250-720 rpm; And / or, the temperature of the first mixing is 20-80°C and the time is 10-14h; and / or, based on 1 g of the silica nanoparticles, the amount of the first solvent is 70-100 mL, and the amount of the alkyl modifier is 1-10 g; and / or, the first solvent is an organic solvent; And / or, the alkyl modifier is an alkyltrialkoxysilane.

12. The composite according to claim 10 or 11, wherein Based on 1 g of the silica nanoparticles, the amount of the alkyl modifier is 1.2-5 g; and / or, the first solvent is at least one of cyclohexane, n-hexane and petroleum ether; And / or, the alkyl modifier is alkyltriethoxysilane and / or alkyltrimethoxysilane.

13. The composite according to claim 12, wherein Alkyl is C 1-18 of normal alkyl.

14. The composite according to claim 13, wherein Alkyl is C 6-14 of normal alkyl.

15. The composite according to claim 1, wherein The weight ratio of the silicon dioxide nanoparticles with alkyl modified surfaces to the acrylamide multi-polymer is 1:5-20.

16. The composite according to claim 15, wherein The weight ratio of the silicon dioxide nanoparticles with surfaces modified by alkyl groups to the acrylamide multi-polymer is 1:10-15.

17. A composite flooding system, characterized in that: The composite flooding system contains the composite according to any one of claims 1 to 16 and a second solvent.

18. The composite profile control and displacement system according to claim 17, wherein: The concentration of the composite in the composite flooding system is 1200-5000 ppm; And / or, the second solvent is water.

19. A method for preparing a composite control and displacement system, characterized in that: The method comprises: In the presence of a second solvent, the silicon dioxide nanoparticles whose surfaces are modified by alkyl groups are mixed with the acrylamide multi-polymer to obtain a composite control and displacement system; The method further comprises the step of preparing the acrylamide multi-polymer: polymerizing the monomer mixture in water under free radical aqueous solution polymerization conditions and in the presence of an initiator; The monomer mixture contains acrylamide, a substance represented by formula I and a substance represented by formula II; Formula I Formula II In formula I, M1 is H, K or Na; In formula II, X is NH; R is selected from C 1-18 Alkyl and / or phenyl.

20. The method according to claim 19, wherein: In formula II, R is C 6-16 Alkyl and / or phenyl.

21. The method according to claim 19, wherein: Based on 100 parts by weight of the monomer mixture, the content of acrylamide is 80-96 parts by weight, the content of the substance represented by formula I is 2-10 parts by weight, and the content of the substance represented by formula II is 2-10 parts by weight.

22. The method according to claim 19, wherein: The initiator is selected from azo initiators and / or redox initiators; And / or, the polymerization reaction is carried out in the presence of a complexing agent and urea.

23. The method according to claim 22, wherein: The initiator is a redox initiator; And / or, the complexing agent is selected from at least one of disodium ethylenediaminetetraacetate, sodium nitrilotriacetate and diethylenetriamine pentacarboxylate; and / or, based on the total weight of the monomer mixture, the amount of urea is 0.01-0.1% by weight; And / or, the weight ratio of the urea to the complexing agent is 1-10:

1.

24. The method according to claim 22, wherein: The redox initiator is selected from at least one of sulfate and sulfite redox initiators, persulfate and thiourea redox initiators, persulfate and organic salt redox initiators, persulfate and sulfite redox initiators, and ammonium persulfate and fatty amine redox initiators; And / or, the complexing agent is selected from at least one of disodium ethylenediaminetetraacetate, sodium nitrilotriacetate and diethylenetriamine pentacarboxylate.

25. The method according to claim 24, wherein: The redox initiator is selected from at least one of sodium sulfate and sodium sulfite, potassium sulfate and potassium sulfite, ammonium sulfate and sodium bisulfite, ammonium sulfate and ammonium sulfite, sodium persulfate and thiourea, potassium persulfate and thiourea, ammonium persulfate and thiourea, sodium persulfate and potassium acetate, potassium persulfate and potassium acetate, ammonium persulfate and ammonium acetate, ammonium persulfate and N,N-tetramethylethylenediamine, and ammonium persulfate and diethylamine; And / or, the complexing agent is disodium ethylenediaminetetraacetate.

26. The method of claim 19, wherein: The polymerization reaction conditions include: temperature of -10°C to 80°C; time of 2-30 hours; pH value of 5-10.

27. The method according to claim 26, wherein: The polymerization reaction conditions include: temperature of 5-60° C.; time of 8-20 hours; and pH value of 6-10.

28. The method of claim 19, wherein: The method further comprises the step of preparing the silica nanoparticles whose surfaces are modified by alkyl groups: In a first solvent, the nano-silica particles are first mixed with an alkyl modifier, and then solid-liquid separation is performed to obtain silica nano-particles with surfaces modified by alkyl groups.

29. The method according to claim 28, wherein: The first mixing is performed under a first stirring condition, and the rotation speed of the first stirring is 250-720 rpm; And / or, the temperature of the first mixing is 20-80°C and the time is 10-14h; and / or, based on 1 g of the nano-silica particles, the amount of the alkyl modifier is 1-10 g; And / or, based on 1 g of the nano-silicon dioxide particles, the amount of the first solvent is 70-100 mL; and / or, the first solvent is an organic solvent; And / or, the alkyl modifier is an alkyltrialkoxysilane.

30. The method of claim 29, wherein: Based on 1g of the nano-silicon dioxide particles, the amount of the alkyl modifier is 1.2-5g; and / or, the first solvent is at least one of cyclohexane, n-hexane and petroleum ether; And / or, the alkyl modifier is alkyltriethoxysilane and / or alkyltrimethoxysilane.

31. The method according to claim 29 or 30, wherein: Alkyl is C 1-18 of normal alkyl.

32. The method according to claim 31, wherein: Alkyl is C 6-14 of normal alkyl.

33. The method of claim 19, wherein: The amounts of the silicon dioxide nanoparticles with alkyl groups modified on the surface and the acrylamide multi-polymer are such that the weight ratio of the silicon dioxide nanoparticles with alkyl groups modified on the surface to the acrylamide multi-polymer is 1:5-20; and / or, the amount of the silicon dioxide nanoparticles with alkyl groups modified on the surface and the acrylamide multi-polymer is such that the total concentration of the silicon dioxide nanoparticles with alkyl groups modified on the surface and the acrylamide multi-polymer in the composite profile control system is 1200-5000 ppm; And / or, the second solvent is water.

34. The method of claim 33, wherein: The amounts of the silicon dioxide nanoparticles with surfaces modified by alkyl groups and the acrylamide multi-polymer are such that the weight ratio of the silicon dioxide nanoparticles with surfaces modified by alkyl groups to the acrylamide multi-polymer is 1:10-15.

35. A method for deep oilfield flooding, characterized in that: The method comprises applying a control and displacement agent to an oil well in an oil field well group, wherein the control and displacement agent is the composite control and displacement system according to claim 17 or 18 or the composite control and displacement system prepared by the method according to any one of claims 19 to 34.