Film forming method and film forming device
By alternately supplying raw material gas and oxygen-containing reaction gas, the plasma ALD method selectively forms oxide films between films of different materials, which solves the difficulty in selectively forming between boron-containing and boron-free films in the prior art. The problem of oxide film achieves better film formation control.
Patent Information
- Application Number
- CN202211326911.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-15
- Filing Date
- 2022-10-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-10-25
AI Technical Summary
The prior art is difficult to selectively form an oxide film between films formed of different materials, especially between a first film containing boron and a second film containing no boron.
By alternately supplying raw material gas containing element X other than halogen and halogen and plasma-containing oxygen-containing reaction gas, an oxide film is selectively formed on the second film by plasma ALD method to ensure that the oxide film is on the second film Formation without forming on the first film.
The selective formation of oxide films between films of different materials is achieved, which improves the film formation control and selectivity of the film, and ensures that the oxide film is mainly formed on the second film without boron.
Smart Images

Figure CN116065139B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a film forming method and a film forming device. Background Art
[0002] The method for forming a nitride film described in Patent Document 1 includes a step of adsorbing chlorine gas on surfaces of a first base film and a second base film, and a step of selectively forming a nitride film on one of the first base film and the second base film on which the chlorine gas is adsorbed.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-174919 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] One embodiment of the present invention provides a technique for forming an oxide film selectively with respect to a first film containing boron on a second film formed of a material different from that of the first film.
[0008] Solutions for solving problems
[0009] A film forming method according to one embodiment of the present disclosure includes the following (A) to (C). (A) A substrate having a first film containing boron and a second film formed of a material different from the material of the first film on its surface is prepared. (B) A raw material gas containing a halogen and an element X other than a halogen is supplied to the surface of the substrate. (C) A plasma-generated reaction gas containing oxygen is supplied to the surface of the substrate. In the film forming method, a third film is selectively formed on the second film relative to the first film by alternately supplying the raw material gas and the plasma-generated reaction gas. The third film is an oxide film of the element X.
[0010] Effects of the Invention
[0011] According to one embodiment of the present disclosure, an oxide film can be formed selectively on a second film formed of a material different from that of the first film with respect to a first film containing boron. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 1 is a flowchart showing a film forming method according to one embodiment.
[0013] Figure 2 This is a diagram showing a first example of the substrate prepared in S101.
[0014] Figure 3This is a diagram showing a second example of the substrate prepared in S101.
[0015] Figure 4 This is a diagram showing a third example of the substrate prepared in S101.
[0016] Figure 5 This is a diagram showing a fourth example of the substrate prepared in S101.
[0017] Figure 6 This is a diagram showing a fifth example of the substrate prepared in S101.
[0018] Figure 7 This is a diagram showing a sixth example of the substrate prepared in S101.
[0019] Figure 8 This is a diagram showing a seventh example of the substrate prepared in S101.
[0020] Fig. 9 This is a flowchart showing an example of S201 to S205 implemented in S101.
[0021] Fig.10 This is a diagram showing an eighth example of the substrate prepared in S101.
[0022] Fig.11 It is a cross-sectional view showing a film forming apparatus according to one embodiment.
[0023] Fig.12 3 is a SEM photograph of the substrate before the treatment of Example 1.
[0024] Fig.13 3 is a SEM photograph of the substrate after the treatment of Example 1.
[0025] Fig.14 3 is a SEM photograph of the substrate before treatment of Example 9.
[0026] Fig.15 3 is a SEM photograph of the substrate after the treatment of Example 9.
[0027] Fig.16 3 is a SEM photograph of the substrate before treatment of Example 13.
[0028] Fig.17 This is a SEM photograph of the substrate after the treatment of Example 13.
[0029] Fig.18 This is a SEM photograph of the substrate of Example 14 before treatment.
[0030] Fig.19 This is a SEM photograph of the substrate after the treatment of Example 14.
[0031] Fig. 20 It is a flowchart which shows the film forming method concerning a modification example.
[0032] Fig.21 It is shown in Fig. 20 Flowchart of the process when K is an integer greater than 2.
[0033] Fig. 22 It is shown Fig.21 FIG. 1 is a diagram of an example of processing of .
[0034] Fig.23 It is shown Fig.21 Figure 2 is a diagram of other processing examples.
[0035] Fig.24 This is a diagram showing a ninth example of the substrate prepared in S101.
[0036] Fig.25 This is a diagram showing a tenth example of the substrate prepared in S101.
[0037] Fig.26 This is a SEM photograph of the substrate of Example 15 before treatment.
[0038] Fig. 27 This is a SEM photograph of the substrate after the treatment of Example 15.
[0039] Fig.28 This is a SEM photograph of the substrate of Example 16 before treatment.
[0040] Fig.29 This is a SEM photograph of the substrate after treatment in Example 16.
[0041] Fig.30 This is a SEM photograph of the substrate before processing of Example 17.
[0042] Fig.31 This is a SEM photograph of the substrate after the treatment of Example 17.
[0043] Fig.32 : is a flowchart showing a film forming method according to the second modification.
[0044] Fig.33 3 is a SEM photograph of the substrate before the treatment of Example 5.
[0045] Fig.34 This is a SEM photograph of the substrate after the treatment of Example 5. DETAILED DESCRIPTION
[0046] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. In addition, in each of the drawings, the same or corresponding structures are denoted by the same reference numerals, and description thereof may be omitted.
[0047] First, refer to Figure 1 The film forming method according to one embodiment is described below. The film forming method includes, for example, Figure 1 The steps S101 to S106 are shown. In addition, the film forming method only needs to include at least steps S101, S102, and S104. The order of steps S102 and S104 can be reversed, and step S104 can be performed before step S102. The film forming method can also include Figure 1 Steps other than steps S101 to S106 shown.
[0048] Figure 1 Step S101 includes preparing a substrate W (refer to Figure 2 ). The substrate W has a first film W1 and a second film W2 on its surface Wa. The first film W1 and the second film W2 are formed on a base substrate (not shown), for example. The base substrate is a silicon wafer or a compound semiconductor wafer. The compound semiconductor wafer is, for example, a GaAs wafer, a SiC wafer, a GaN wafer, or an InP wafer.
[0049] The first film W1 contains boron (B). The B content in the first film W1 is, for example, 20 atomic % to 100 atomic %, preferably 40 atomic % to 100 atomic %. The first film W1 is, for example, a B film, a BN film, a BNC film, a BO film, a BNOC film, a SiBN film, a SiBCN film, or a SiOBN film. Here, the BN film refers to a film containing boron (B) and nitrogen (N). The atomic ratio of B to N in the BN film is not limited to 1:1. BNC films other than BN films also refer to films containing each element, and there is no limitation on the stoichiometric ratio.
[0050] The second film W2 is formed of a material different from that of the first film W1. The second film W2 does not substantially contain B. Substantially containing no B means that the B content is 0 atomic % to 5 atomic %. The smaller the B content in the second film W2, the better. The second film W2 may be any of an insulating film, a conductive film, and a semiconductor film.
[0051] There is no particular limitation on the insulating film, and examples thereof include SiO film, SiN film, SiOC film, SiON film, SiOCN film, AlO film, ZrO film, HfO film or TiO film. Here, SiO film refers to a film containing silicon (Si) and oxygen (O). The atomic ratio of Si to O in the SiO film is generally 1:2, but is not limited to 1:2. SiN film, SiOC film, SiON film, SiOCN film, AlO film, ZrO film, HfO film and TiO film also refer to films containing various elements, and there is no limitation on the stoichiometric ratio. The insulating film is, for example, an interlayer insulating film. The interlayer insulating film is preferably a low dielectric constant (Low-k) film.
[0052] The semiconductor film is not particularly limited, and may be, for example, a Si film, a SiGe film, or a GaN film. The semiconductor film may be any of a single crystal film, a polycrystalline film, and an amorphous film.
[0053] The conductive film is, for example, a metal film. There is no particular limitation on the metal film, and examples thereof include a Cu film, a Co film, a Ru film, a Mo film, a W film, or a Ti film. The conductive film may also be a metal nitride film. There is no particular limitation on the metal nitride film, and examples thereof include a TiN film or a TaN film. Here, the TiN film refers to a film containing titanium (Ti) and nitrogen (N). The atomic ratio of Ti to N in the TiN film is generally 1:1, but is not limited to 1:1. The TaN film also refers to a film containing each element, and there is no limitation on the stoichiometric ratio.
[0054] Figure 1 Step S102 includes supplying a raw material gas to the surface Wa of the substrate W. The raw material gas contains halogens and elements X other than halogens. Halogens are fluorine, chlorine, bromine or iodine. Element X is not particularly limited as long as it is an element that will be oxidized in step S104, but is preferably a metal element, more preferably a transition metal element. Transition metal elements are, for example, Ti, W, V, Al, Mo, Sn or Hf. As specific examples of raw material gas, TiCl4 gas, WCl6 gas, VCl4 gas, AlCl3 gas, MoCl5 gas, SnCl4 gas or HfCl4 gas can be listed. Element X can be a semiconductor element, specifically, Si or Ge. The raw material gas is a silicon halide gas or a germanium halide gas. As specific examples of silicon halide gas, SiCl4 gas, SiHCl3 gas, SiH2Cl2 gas, SiH3Cl gas, Si2Cl6 gas, Si2HCl5 gas, SiH2I2 gas or SiCl3CH3 gas can be listed. Specific examples of germanium halide gas include GeCl4 gas, etc. The raw material gas may be supplied together with a diluent gas, such as Ar gas or N2 gas.
[0055] Figure 1 Step S103 includes supplying a purge gas to the surface Wa of the substrate W. The purge gas purges the remaining source gas that is not adsorbed to the surface Wa of the substrate W in the above step S102. As the purge gas, for example, a rare gas such as Ar gas or N2 gas can be used.
[0056] Figure 1 Step S104 includes supplying a reaction gas to the surface Wa of the substrate W. Step S104 includes converting the reaction gas into plasma and supplying the plasma-converted reaction gas to the surface Wa of the substrate W. The reaction gas contains oxygen and oxidizes the element X contained in the adsorbed raw material gas to form an oxide film of the element X, that is, a third film W3 (see Figure 2). The reaction gas is, for example, O2 gas, O3 gas, CO2 gas, N2O gas, NO gas or H2O gas. The reaction gas may be supplied together with a diluent gas. The diluent gas is, for example, Ar gas or N2 gas.
[0057] In addition, the reaction gas may be supplied not only in the above step S104 but also in all steps S102 to S105. However, the reaction gas is converted into plasma only in the above step S104. This is because the reaction gas is easily reacted with the raw material gas adsorbed on the surface Wa of the substrate W by being converted into plasma.
[0058] Figure 1 Step S105 includes supplying a purge gas to the surface Wa of the substrate W. The purge gas purges the remaining reaction gas that has not reacted with the surface Wa of the substrate W in the above step S104. As the purge gas, for example, a rare gas such as Ar gas or N2 gas can be used.
[0059] exist Figure 1 In step S106, it is confirmed whether the above steps S102 to S105 have been performed N times (N is an integer greater than 1). N may be an integer greater than 2, and the above steps S102 to S105 may be repeatedly performed. The film thickness of the third film W3 can be increased.
[0060] When the number of executions of the above steps S102 to S105 is less than N times (step S106, "No"), the film thickness of the third film W3 is less than the target value, so the above steps S102 to S105 are executed again. N is preferably 200 or more, more preferably 300 or more. N is preferably 1000 or less.
[0061] On the other hand, when the number of executions of the above-mentioned steps S102 to S105 reaches N times (step S106 , “Yes”), the film thickness of the third film W3 reaches the target value, and thus the current processing is terminated.
[0062] According to the present embodiment, the third film W3 is selectively formed on the second film W2 relative to the first film W1 by a plasma ALD (Atomic Layer Deposition) method. In order to selectively form the third film W3, it is important that the raw material gas is weakly adsorbed relative to the first film W1, and the raw material gas adsorbed on the first film W1 is separated without undergoing a film forming reaction (formation of the third film W3) by collision or reaction with the plasma-formed reaction gas.
[0063] The ease with which the raw material gas adsorbed on the first film W1 can be released varies depending on the adsorption strength of the raw material gas relative to the first film W1 and varies depending on the material of the first film W1. The ease with which the raw material gas adsorbed on the first film W1 can be released varies depending on whether the raw material gas is dissociated through a reaction with atoms on the surface of the first film W1 and becomes a molecule that is easily oxidized in a subsequent reaction. It is believed that, compared with the second film W2 that does not substantially contain boron, on the first film W1 containing boron, the adsorption of the halide as the raw material gas is weaker or does not occur, or the dissociation of the halide is less likely to occur.
[0064] Oxygen ions or oxygen free radicals are generated by plasma-forming the reaction gas containing oxygen. The oxygen ions are accelerated by the potential based on the plasma and collide with the substrate W. It is believed that sputtering that physically blasts out the substance on the surface Wa occurs due to the collision of the accelerated oxygen ions or oxygen free radicals. In addition, it is also believed that film formation occurs due to the chemical reaction between the oxygen ions or oxygen free radicals and the substance on the surface Wa.
[0065] The halide adsorbed on the second film W2 that does not substantially contain boron is strongly adsorbed or dissociated into molecules that are easily oxidized, and is easily oxidized by collision with oxygen ions or oxygen radicals. Therefore, it is considered that an oxide film is formed on the second film W2. On the other hand, the halide adsorbed on the first film W1 containing boron is weakly adsorbed or does not dissociate into molecules that are easily oxidized, and is therefore ejected by collision with oxygen ions or oxygen radicals. Therefore, it is considered that an oxide film is not formed on the first film W1.
[0066] The reason why the oxide film is not formed on the first film W1 is that the halide is released by sputtering or chemical reaction, or the first film W1 is etched by collision of oxygen ions or oxygen radicals, thereby peeling off the halide.
[0067] In addition, if Fig.32 As shown, step S109 may be performed instead of step S104. Step S109 includes supplying O3 gas to the surface Wa of the substrate W in a manner that does not convert the O3 gas into plasma. Since the O3 gas is supplied in a manner that does not convert the O3 gas into plasma, it does not contain oxygen ions and oxygen free radicals at first. The O3 gas collides with the surface Wa of the heated substrate W to generate oxygen free radicals. The oxygen free radicals oxidize the halides adsorbed on the second film W2 that does not substantially contain boron, so that the formation of the oxide film progresses. On the other hand, the halides adsorbed on the first film W1 that contains boron are blasted out, thereby preventing the formation of the oxide film.
[0068] In addition, by converting a reaction gas that does not contain oxygen, such as H2 gas or NH3 gas, into plasma, active species such as ions or radicals are also generated, but these active species easily cause the film forming reaction to proceed. Therefore, it is considered that when a reaction gas that does not contain oxygen is used, the film forming reaction is likely to proceed not only on the second film W2 but also on the first film W1, thereby impairing the selectivity. Therefore, as the gas to be converted into plasma, a gas containing oxygen is suitable.
[0069] In addition, the halide adsorbed on the first film W1 is not easily decomposed by the collision of oxygen ions or oxygen free radicals. For example, compared with organic metal complexes such as Ti[N(CH3)2]4, halides such as TiCl4 are not easily decomposed by the collision of oxygen ions or oxygen free radicals. In order to make the halide adsorbed on the first film W1 detach from the first film W1, it is important that it is not easily decomposed by the collision of oxygen ions or oxygen free radicals and the heat from the substrate. Therefore, as a raw material gas, a halogen-containing gas is suitable.
[0070] Furthermore, in the plasma CVD (Chemical Vapor Deposition) method, which converts halides and oxygen into plasma, active species such as ions or radicals generated by dissociation of halides are generated in addition to oxygen ions or oxygen radicals. It is believed that the active species generated from the halides are highly reactive and are likely to undergo film-forming reactions not only on the second film W2 but also on the first film W1, thereby impairing selectivity. In order to generate selectivity, it is important to use the plasma ALD method.
[0071] In the above steps S102 to S105, the temperature of the substrate W may be controlled to be above 100°C in order to promote the separation of the raw material gas from the first film W1. When the temperature of the substrate W is lower than 100°C, the separation of the raw material gas is not sufficiently caused on the first film W1, resulting in physical adsorption of the raw material gas, so that the third film W3 is formed on the entire surface Wa of the substrate W. The temperature of the substrate W is preferably above 300°C. The temperature of the substrate W is preferably below 800°C.
[0072] Next, refer to Figure 3 to Figure 5 The following describes a case where the substrate W prepared in step S101 has a concave portion Wa1 on the surface Wa, and the second film W2 is exposed only inside the concave portion Wa1. Figure 3 to Figure 5 As shown, the second film W2 is exposed at least on the bottom surface of the recess Wa1. In this case, by performing steps S102 to S106, the third film W3 can be filled inside the recess Wa1. Figure 3 to Figure 5 In the embodiment, the third film W3 fills a part of the recess Wa1, but the entire recess Wa1 may be filled. Figure 5In the embodiment, etching can be performed so that the first film W1 remains only on the top surface of the convex portion of the second film W2.
[0073] exist Figure 3 In step S101, first, the first film W1 is formed on the entire surface of the second film W2, and then a portion of the surface of the first film W1 is etched. As a result, a recess Wa1 is formed in a manner that penetrates a portion of the first film W1, and the second film W2 is exposed only on the bottom surface of the recess Wa1. Thereafter, by implementing steps S102 to S106, the third film W3 is grown only on the bottom surface of the recess Wa1.
[0074] exist Figure 4 In step S101, first, a portion of the surface of the second film W2 is etched to form a recess on the surface of the second film W2. Then, a first film W1 is formed to fill the recess. Next, the first film W1 is processed by CMP (Chemical Mechanical Polishing) or etching until the second film W2 is exposed. Finally, the second film W2 is selectively etched relative to the first film W1. As a result, a recess Wa1 is formed in a manner that penetrates a portion of the first film W1, and the second film W2 is exposed only on the bottom surface of the recess Wa1. Thereafter, by implementing steps S102 to S106, a third film W3 is grown only on the bottom surface of the recess Wa1.
[0075] exist Figure 5 In step S101, first, a portion of the surface of the second film W2 is etched to form a recessed portion on the surface of the second film W2. Next, the first film W1 is selectively formed on the outside of the recessed portion (i.e., the top surface of the convex portion) relative to the inside of the recessed portion. As a result, the second film W2 is exposed at the bottom surface and the lower part of the side surface of the recessed portion Wa1. In addition, if the first film W1 is also deposited on the bottom surface of the recessed portion Wa1 in the middle of step S101, the first film W1 deposited on the bottom surface is removed by etching or the like. Thereafter, by implementing steps S102 to S106, a third film W3 is grown at the bottom surface and the lower part of the side surface of the recessed portion Wa1.
[0076] Next, refer to Figure 6 to Figure 8 The following describes a case where the substrate W prepared in step S101 has a concave portion Wa1 on the surface Wa, and the first film W1 is exposed only inside the concave portion Wa1. Figure 6 to Figure 8 As shown, the first film W1 is exposed at least on the bottom surface of the recess Wa1. In this case, by performing steps S102 to S106, the third film W3 can be formed other than the bottom surface of the recess Wa1.
[0077] exist Figure 6In step S101, first, the second film W2 is formed on the entire surface of the first film W1, and then a portion of the surface of the second film W2 is etched. As a result, a recess Wa1 is formed in a manner that penetrates a portion of the second film W2, and the first film W1 is exposed only at the bottom of the recess Wa1. Then, by implementing steps S102 to S106, a third film W3 is grown on the side of the recess Wa1 and the outside of the recess Wa1 (the top surface of the convex portion).
[0078] exist Figure 7 In step S101, first, a portion of the surface of the first film W1 is etched to form a recess on the surface of the first film W1. Then, a second film W2 is formed to fill the recess. Next, the second film W2 is processed by CMP (Chemical Mechanical Polishing) or etching until the first film W1 is exposed. Finally, the first film W1 is selectively etched relative to the second film W2. As a result, a recess Wa1 is formed in a manner that penetrates a portion of the second film W2, and the first film W1 is exposed only on the bottom surface of the recess Wa1. Thereafter, by implementing steps S102 to S106, a third film W3 is grown on the side of the recess Wa1 and the outside of the recess Wa1 (the top surface of the convex portion).
[0079] exist Figure 8 In step S101, first, a portion of the surface of the first film W1 is etched to form a recessed portion on the surface of the first film W1. Next, a second film W2 is selectively formed on the outside of the recessed portion (i.e., the top surface of the convex portion) relative to the inside of the recessed portion. As a result, the first film W1 is exposed at the bottom surface and the lower portion of the side surface of the recessed portion Wa1. In addition, if the second film W2 is also deposited on the bottom surface of the recessed portion Wa1 in the middle of step S101, the second film W2 deposited on the bottom surface is removed by etching or the like. Thereafter, by implementing steps S102 to S106, a third film W3 is grown on the outside of the recessed portion Wa1 (i.e., the top surface of the convex portion) and the upper portion of the side surface of the recessed portion Wa1. As shown in FIG. Figure 8 As shown, the third film W3 can close the void (air gap) inside the recess Wa1.
[0080] Next, refer to Figure 9-10 A variation of step S101 is described below. Fig.10 As shown, step S101 may include: selectively forming the first film W1 on the fourth film W4 formed of a material different from that of the second film W2 relative to the second film W2. As described above, the first film W1 contains boron.
[0081] The fourth film W4 may be any one of an insulating film, a conductive film, and a semiconductor film as long as it can selectively form the first film W1 on the fourth film W4 relative to the second film W2. For example, the incubation time of the first film W1 relative to the second film W2 may be longer than the incubation time of the first film W1 relative to the fourth film W4. The first film W1 can be selectively formed by utilizing the difference in incubation time.
[0082] The incubation time is the time difference from the start of the film formation process (for example, the start of supply of a raw material gas or a reaction gas) to the actual start of film formation.
[0083] Step S101 includes, for example: Fig. 9 Steps S201 to S205 are shown. In addition, step S101 may include at least steps S201 and S203. The order of steps S201 and S203 may be reversed, or step S203 may be performed before step S201. Steps S201 and S203 may be performed simultaneously, or the CVD method may be used.
[0084] Fig. 9 Step S201 includes supplying a second source gas to the surface of the substrate W. The second source gas contains boron. The second source gas, for example, contains tris(dimethylamino)borane (TDMAB: C6H 18 BN3). The second raw material gas may be supplied together with a diluent gas. The diluent gas is, for example, Ar gas or N2 gas.
[0085] In addition, the second raw material gas is not limited to containing TDMAB, as long as it contains boron. For example, it can also contain diborane (B2H6), boron trichloride (BCl3), boron trifluoride (BF3), triethylmethylaminoborane (C9H 24 BN3), trimethylborane (C3H9B), or triethylborane (C6H 15 B), borohydride (B3N3H6), etc.
[0086] Fig. 9 Step S202 includes supplying a purge gas to the surface of the substrate W. The purge gas purges the remaining second source gas that is not adsorbed on the surface Wa of the substrate W in the above step S201. As the purge gas, for example, a rare gas such as Ar gas or N2 gas can be used.
[0087] Fig. 9 Step S203 includes supplying a second reaction gas to the surface of the substrate W. The second reaction gas contains nitrogen, for example, and forms a first film W1 (for example, a BN film) by nitriding the adsorbed second raw material gas. The second reaction gas contains, for example, a mixed gas of N2 gas and H2 gas, or NH3 gas. The second reaction gas may be supplied together with a dilution gas. The dilution gas is, for example, Ar gas or N2 gas.
[0088] In addition, the second reaction gas may include at least one of a nitrogen-containing gas, an oxygen-containing gas, and a reducing gas. The nitrogen-containing gas forms a boron nitride film by nitriding the second raw material gas. The nitrogen-containing gas may include, for example, NH3, N2, N2H4, or N2H2. The oxygen-containing gas may form a boron oxide film by oxidizing the second raw material gas. The oxygen-containing gas may include, for example, O2, O3, H2O, NO, or N2O. The reducing gas may form a boron film by reducing the second raw material gas. The reducing gas may include, for example, H2 or SiH4.
[0089] Step S203 may include converting the second reaction gas into plasma, or may include supplying the second reaction gas converted into plasma to the surface Wa of the substrate W. By converting the second reaction gas into plasma, the formation of the first film W1 can be promoted.
[0090] In addition, the second reaction gas may be supplied not only in step S203 but also in all steps S201 to S204. However, the second reaction gas is converted into plasma only in step S203. This is because the reaction between the second reaction gas and the second source gas adsorbed on the surface of the substrate W is promoted by converting the second reaction gas into plasma.
[0091] Fig. 9 Step S204 includes supplying a purge gas to the surface of the substrate W. The purge gas purges the remaining second reaction gas that has not reacted with the surface Wa of the substrate W in the above step S203. As the purge gas, for example, a rare gas such as Ar gas or N2 gas can be used.
[0092] exist Fig. 9 In step S205, it is confirmed whether the above steps S201 to S204 have been performed M times (M is an integer greater than or equal to 1). M may be an integer greater than or equal to 2, and the above steps S201 to S204 may be repeatedly performed. The film thickness of the first film W1 can be increased.
[0093] If the number of executions of the above steps S201 to S204 is less than M times (step S205, "No"), the film thickness of the first film W1 is less than the target value, and therefore the above steps S201 to S204 are executed again. The target value of the film thickness of the first film W1 is preferably The following are more preferably The following is further preferably The following. It can also be about film thickness.
[0094] On the other hand, when the number of executions of the above steps S201 to S204 reaches M times (step S205 , “Yes”), the film thickness of the first film W1 has reached the target value, and thus the current processing is terminated.
[0095] also, Fig. 9 The formation method of the first film W1 shown is the ALD method, but it can also be the CVD method. In the ALD method, the supply of the second raw material gas and the supply of the second reaction gas are alternately performed. On the other hand, in the CVD method, the supply of the second raw material gas and the supply of the second reaction gas are simultaneously performed.
[0096] In addition, the first film W1 can also be a molecular film with chemically adsorbed molecules such as a self-assembled monolayer (SAM). The molecules are supplied to the substrate surface in a gaseous or liquid state. The molecules have a first functional group that is selectively chemically adsorbed to a desired area on the substrate surface. There is no particular limitation on the first functional group, and examples include a thiol group (SH group), a carboxyl group (COOH group), or a hydroxyl group (OH group). In addition to the first functional group, the molecule also includes a second functional group containing B. The second functional group is a functional group such as BH3 or B(CH3)3 in which at least a portion of the carbon of the hydrocarbon group is replaced by boron (B). The first film W1 can also be a film obtained by thermally decomposing the molecular film.
[0097] Next, refer to Fig. 20 The film forming method involved in the modification example is described below. Fig. 20 As shown, the film forming method of this variation includes step 301 , steps S201 to S205 , steps S102 to S106 , and step S302 .
[0098] Fig. 20 Steps S201 to S205 in Fig. 9 Steps S201 to S205 in the above are the same, so their description is omitted. In addition, the film forming method may not include all of the steps S201 to S205. It is sufficient as long as the first film W1 can be selectively formed in a desired region.
[0099] in addition, Fig. 20 Steps S102 to S106 in Figure 1 Since steps S102 to S106 are the same as those in the above, the description thereof is omitted. In addition, the film forming method may not include all steps S102 to S106. It is sufficient as long as the third film W3 can be selectively formed in a desired region.
[0100] Step S301 includes preparing a substrate W having a second film W2 and a fourth film W4 on a surface Wa (see Fig. 22). Then, through steps S201 to S205, the first film W1 is selectively formed on the fourth film W4 relative to the second film W2. And, then, through steps S102 to S106, the third film W3 is selectively formed on the second film W2 relative to the first film W1.
[0101] Step S302 includes confirming whether a series of processes have been performed K times (K is an integer greater than 1). A series of processes includes: performing steps S201 to S204 M times (M is an integer greater than 1); and performing steps S102 to S105 N times (N is an integer greater than 1).
[0102] When the number of implementations is less than K times (step S302, "No"), the film thickness of the third film W3 is insufficient, so the control unit 100 performs a series of processes again. On the other hand, when the number of implementations reaches K times (step S302, "Yes"), the control unit 100 ends the current process. K is preferably an integer greater than 2. If K is an integer greater than 2, the film thickness of the third film W3 can be increased while supplementing the first film W1.
[0103] Next, refer to Figure 21 to Figure 23 The film forming method will be described below when K is an integer greater than 2. Fig.21 As shown, the film forming method may include steps S401 to S405. Fig.21 , L is equal to (K-1).
[0104] Step S401 includes, similarly to step S301, preparing a substrate W having a second film W2 and a fourth film W4 on a surface Wa (see Fig. 22 The fourth film W4 only needs to be able to selectively form the first film W1 on the fourth film W4 relative to the second film W2. For example, the incubation time of the first film W1 relative to the second film W2 is longer than the incubation time of the first film W1 relative to the fourth film W4.
[0105] Step S402 includes forming a first film W1 selectively on a fourth film W4 relative to the second film W2 (see Fig. 22 ). Step S402 includes performing steps S201 to S204 M times. M is an integer greater than 1. M can be an integer greater than 2.
[0106] Step S403 includes forming a third film W3 (see FIG. 1 ) selectively on the second film W2 relative to the first film W1. Fig. 22 ). Step S403 includes performing steps S102 to S105 N times. N is an integer greater than 1. N can be an integer greater than 2.
[0107] Step S404 includes forming the first film W1 again on the first film W1 selectively relative to the third film W3 (refer to Fig. 22 ). Step S404, like step S402, includes: performing steps S201 to S204 M times.
[0108] In addition, in the process of forming the third film W3 in step S403, the first film W1 may become thinner or disappear (see Fig.23 ). In the case where the first film W1 disappears, step S404 includes selectively forming the first film W1 again on the fourth film W4 instead of the first film W1 (refer to Fig.23 ).
[0109] Step S405 includes forming the third film W3 again on the third film W3 selectively with respect to the first film W1. Step S405 includes performing steps S102 to S105 N times, similarly to step S403.
[0110] Step S406 includes confirming whether steps S404 to S405 have been performed L times (L = (K-1)). If the number of times performed is less than L times (step S406, "No"), the control unit 100 performs steps S404 to S405 again. On the other hand, if the number of times performed reaches L times (step S406, "Yes"), the control unit 100 ends the current processing.
[0111] Next, refer to Fig.24 Other variations of step S101 are described below. Fig.24 In step S101, first, a second film W2 having a concave-convex pattern is prepared. Then, the first film W1 is formed on the entire second film W2 along the concave-convex pattern of the second film W2 by the ALD method or the CVD method. Then, the top surface of the convex portion of the second film W2 is exposed by CMP or etching. At this time, the first film W1 remains on the side and bottom surface of the concave portion of the second film W2. Thereafter, by implementing steps S102 to S106, the third film W3 can be formed on the top surface of the convex portion.
[0112] Next, refer to Fig.25 Another example of step S101 is described below. Fig.25In step S101, first, a second film W2 having a concave-convex pattern is prepared. Then, a first film W1 is formed to fill the concave portion of the second film W2. The first film W1 is a liquid. The liquid is, for example, a liquid formed by polymerizing B-containing molecules having organic ligands such as TDMAB by N2 plasma or the like. Next, the liquid buried in the concave portion of the second film W2 is decomposed by O2 plasma or the like, and the first film W1 remains on the side and bottom surfaces of the concave portion of the second film W2. The top surface of the convex portion of the second film W2 remains exposed. The liquid buried in the concave portion of the second film W2 can also be modified by H2 plasma or the like, thereby forming the first film W1 buried in the concave portion of the second film W2, but this is not shown in the figure. Thereafter, by implementing steps S102 to S106, a third film W3 can be formed on the top surface of the convex portion.
[0113] Next, refer to Fig.11 The film forming apparatus 1 is described below. The film forming apparatus 1 includes a substantially cylindrical airtight processing container 2. An exhaust chamber 21 is provided at the center of the bottom wall of the processing container 2. The exhaust chamber 21 has a shape, for example, substantially cylindrical, protruding downward. An exhaust pipe 22 is connected to the exhaust chamber 21, for example, at the side of the exhaust chamber 21.
[0114] The exhaust pipe 22 is connected to the exhaust section 24 via a pressure regulating section 23. The pressure regulating section 23 includes a pressure regulating valve such as a butterfly valve. The exhaust pipe 22 is configured to reduce the pressure in the processing container 2 through the exhaust section 24. A transfer port 25 is provided on the side of the processing container 2. The transfer port 25 is opened and closed by a gate valve 26. The substrate W is transferred in and out between the processing container 2 and the transfer chamber (not shown) via the transfer port 25.
[0115] A loading table 3 is provided in the processing container 2. The loading table 3 is a holding portion that holds the substrate W horizontally in a manner in which the surface Wa of the substrate W faces upward. The loading table 3 is formed to be roughly circular in a plan view and is supported by a supporting member 31. A roughly circular recess 32 for mounting a substrate W having a diameter of, for example, 300 mm is formed on the surface of the loading table 3. The recess 32 has an inner diameter slightly larger than the diameter of the substrate W. The depth of the recess 32 is, for example, configured to be roughly the same as the thickness of the substrate W. The loading table 3 is formed of, for example, a ceramic material such as aluminum nitride (AlN). In addition, the loading table 3 can also be formed of a metal material such as nickel (Ni). In addition, a guide ring for guiding the substrate W can also be provided on the peripheral portion of the surface of the loading table 3 instead of the recess 32.
[0116] A grounded lower electrode 33 is embedded in the stage 3, for example. A heating mechanism 34 is embedded below the lower electrode 33. The heating mechanism 34 is powered by a power supply unit (not shown) based on a control signal from the control unit 100, thereby heating the substrate W mounted on the stage 3 to a set temperature. In the case where the stage 3 is entirely made of metal, the stage 3 functions as a lower electrode as a whole, so the lower electrode 33 may not be embedded in the stage 3. A plurality of (for example, three) lifting pins 41 are provided in the stage 3 for holding the substrate W mounted on the stage 3 and lifting the substrate W. The material of the lifting pins 41 may be, for example, ceramics such as alumina (Al2O3), quartz, etc. The lower ends of the lifting pins 41 are mounted on a support plate 42. The support plate 42 is connected to a lifting mechanism 44 disposed outside the processing container 2 via a lifting shaft 43.
[0117] The lifting mechanism 44 is provided, for example, at the lower part of the exhaust chamber 21. The bellows 45 is provided between the opening 211 for the lifting shaft 43, which is formed at the lower surface of the exhaust chamber 21, and the lifting mechanism 44. The support plate 42 may be shaped so as to be able to be lifted and lowered without interfering with the support member 31 of the mounting table 3. The lifting pin 41 is configured to be lifted and lowered between the upper surface of the mounting table 3 and the lower surface of the mounting table 3 by the lifting mechanism 44.
[0118] A gas supply unit 5 is provided on the top wall 27 of the processing container 2 via an insulating member 28. The gas supply unit 5 forms an upper electrode and faces the lower electrode 33. The gas supply unit 5 is connected to a high-frequency power supply 512 via a matcher 511. By supplying a high-frequency power of 100kHz to 2.45GHz, preferably 450kHz to 100MHz, from the high-frequency power supply 512 to the upper electrode (gas supply unit 5), a high-frequency electric field is generated between the upper electrode (gas supply unit 5) and the lower electrode 33, thereby generating capacitively coupled plasma. The plasma generating unit 51 includes a matcher 511 and a high-frequency power supply 512. In addition, the plasma generating unit 51 is not limited to generating capacitively coupled plasma, and other plasmas such as inductively coupled plasma can also be generated. In addition, the plasma-formed gas can also be supplied from a remote plasma source.
[0119] The gas supply unit 5 includes a hollow gas supply chamber 52. A plurality of holes 53 for distributing and supplying the processing gas into the processing container 2 are evenly arranged on the lower surface of the gas supply chamber 52, for example. A heating mechanism 54 is buried in the gas supply unit 5, for example, above the gas supply chamber 52. The heating mechanism 54 is supplied with power from a power supply unit (not shown) based on a control signal from the control unit 100, and is thereby heated to a set temperature.
[0120] The gas supply path 6 is provided in the gas supply chamber 52. The gas supply path 6 is connected to the gas supply chamber 52. Gas sources G61, G62, and G63 are connected to the upstream of the gas supply path 6 via gas lines L61, L62, and L63, respectively. In addition, the number of gas sources and the types of gases are not limited to those shown in the figure.
[0121] The gas source G61 is a gas source of TiCl4 and is connected to the gas supply path 6 via a gas line L61. In the gas line L61, a mass flow controller M61, a storage tank T61, and a valve V61 are provided in the order of a mass flow controller M61, a storage tank T61, and a valve V61 from the gas source G61 side. The mass flow controller M61 controls the flow rate of the TiCl4 gas flowing in the gas line L61. The storage tank T61 can store the TiCl4 gas supplied from the gas source G61 via the gas line L61 in a state where the valve V61 is closed to increase the pressure of the TiCl4 gas in the storage tank T61. The valve V61 performs the supply / cutoff of the TiCl4 gas relative to the gas supply path 6 by opening and closing.
[0122] The gas source G62 is a gas source of Ar, and is connected to the gas supply path 6 via a gas line L62. In the gas line L62, a mass flow controller M62 and a valve V62 are provided in the order of the mass flow controller M62 and the valve V62 from the gas source G62 side. The mass flow controller M62 controls the flow rate of the Ar gas flowing in the gas line L62. The valve V62 supplies / cuts off the Ar gas to the gas supply path 6 by opening and closing.
[0123] The gas source G63 is a gas source of O2 and is connected to the gas supply path 6 via a gas line L63. In the gas line L63, a mass flow controller M63 and a valve V63 are provided in the order of the mass flow controller M63 and the valve V63 from the gas source G63 side. The mass flow controller M63 controls the flow rate of the O2 gas flowing in the gas line L63. The valve V63 supplies / cuts off the O2 gas to the gas supply path 6 by opening and closing.
[0124] The film forming apparatus 1 includes a control unit 100 and a storage unit 101. The control unit 100 includes a CPU, a RAM, a ROM, etc. (none of which are shown in the figure), and controls the film forming apparatus 1 in a unified manner by, for example, causing the CPU to execute a computer program stored in the ROM or the storage unit 101. Specifically, the control unit 100 controls the operation of each component of the film forming apparatus 1 by causing the CPU to execute a control program stored in the storage unit 101, thereby performing a film forming process on the substrate W, etc.
[0125] Next, refer to Fig.11The operation of the film forming apparatus 1 will be described. First, the control unit 100 opens the gate valve 26, and transports the substrate W into the processing container 2 and places it on the mounting table 3 through the transport mechanism. The substrate W is placed horizontally with the surface Wa facing upward. The control unit 100 causes the transport mechanism to withdraw from the processing container 2, and then closes the gate valve 26. Next, the control unit 100 heats the substrate W to a set temperature through the heating mechanism 34 of the mounting table 3, and adjusts the pressure in the processing container 2 to a set pressure through the pressure adjustment unit 23. For example, Figure 1 The step S101 includes carrying the substrate W into the processing container 2 and the like.
[0126] Next, the control unit 100 implements Figure 1 In step S102, valves V61, V62, and V63 are opened to supply TiCl4 gas, Ar gas, and O2 gas into the processing container 2 simultaneously.
[0127] The specific processing conditions of the above-mentioned step S102 are as follows, for example.
[0128] TiCl4 gas flow rate: 1sccm~500sccm
[0129] Ar gas flow rate: 100 sccm~100000 sccm
[0130] O2 gas flow rate: 100sccm~100000sccm
[0131] Processing time: 0.1 seconds to 30 seconds
[0132] Processing temperature: 100℃~450℃
[0133] Processing pressure: 3Pa~10000Pa.
[0134] Next, the control unit 100 implements Figure 1 In step S103, the valve V61 is closed. At this time, since the valves V62 and V63 are open, the Ar gas and the O2 gas are supplied into the processing container 2, and the TiCl4 gas remaining in the processing container 2 is exhausted to the exhaust pipe 22.
[0135] The specific processing conditions of the above-mentioned step S103 are as follows, for example.
[0136] Ar gas flow rate: 100 sccm~100000 sccm
[0137] O2 gas flow rate: 100sccm~100000sccm
[0138] Processing time: 0.1 seconds to 30 seconds
[0139] Processing temperature: 100℃~450℃
[0140] Processing pressure: 3Pa~10000Pa.
[0141] Next, the control unit 100 implements Figure 1 In step S104, plasma is generated by the plasma generating unit 51 to convert the O2 gas into plasma. As a result, the adsorbed TiCl4 gas is oxidized, for example, to form a TiO film. The TiO film is selectively formed on the second film W2 relative to the first film W1. The specific processing conditions of step S104 other than the generation of plasma are the same as those of the above-mentioned step S103, and thus the description thereof is omitted.
[0142] Next, the control unit 100 implements Figure 1 In step S105, the generation of plasma is stopped. At this time, since valves V62 and V63 are open, Ar gas and O2 gas are supplied into the processing container 2, and the plasma-generated gas remaining in the processing container 2 is exhausted to the exhaust pipe 22. The specific processing conditions of step S105 are the same as those of the above-mentioned step S103, so the description is omitted.
[0143] Then, in Figure 1 In step S106, the control unit 100 confirms whether steps S102 to S105 have been implemented N times (N is a natural number greater than 1). When the number of implementations is less than N times (step S106, "No"), the control unit 100 implements steps S102 to S105 again. On the other hand, when the number of implementations reaches N times (step S106, "Yes"), the control unit 100 ends the current processing. Thereafter, the control unit 100 opens the gate valve 26 and transports the substrate W to the outside of the processing container 2 through the transport mechanism. The control unit 100 causes the transport mechanism to retreat from the processing container 2, and then closes the gate valve 26.
[0144] In addition, the control unit 100 may also implement Fig. 9 In addition, the control unit 100 may also implement steps S201 to S205. Fig. 20 The series of processing shown. The series of processing includes: performing steps S201 to S204 M times (M is an integer greater than 1); and performing steps S102 to S105 N times (N is an integer greater than 1). The control unit 100 performs the series of processing K times (K is an integer greater than 1).
[0145] In addition, Figure 1In the embodiment, steps S102 to S105 are performed N times, but as shown in Table 12 described later, steps S102A and S103A may be performed after step S103 and before step S104. Step S102A is performed in the same manner as step S102 except that a different raw material gas is used from step S102. Step S103A is performed in the same manner as step S103.
[0146] As shown in Table 12 described later, by repeatedly supplying a raw material gas containing an element X1 as the element X, supplying a raw material gas containing an element X2 as the element X which is different from the element X1, and supplying a plasma-generated reaction gas, an oxide film of the element X (to be specific, the elements X1 and X2), that is, a third film W3, can be selectively formed on the second film W2 relative to the first film W1. Either the element X1 or the element X2 is a metal element (preferably a transition metal element), and the other is a semiconductor element. By performing both steps S102 and S102A, crystallization of the third film W3 can be suppressed, and the flatness of the third film W3 can be improved.
[0147] In addition, in Table 12, element X1 is a metal element and element X2 is a semiconductor element, but element X1 may be a semiconductor element and element X2 may be a metal element. In addition, the combination of element X1 and element X2 may be a combination of metal elements or a combination of semiconductor elements. Element X may include element X3 different from elements X1 and X2, or may include three or more different elements. The control unit 100 may also implement the supply of a raw material gas including element X3.
[0148] In addition, as shown in Table 13 described later, steps S102A to S105A may be performed after the nth (n is any natural number greater than 1 and less than N) steps S102 to S105 and before the n+1th steps S102 to S105. Step S102A is performed in the same manner as step S102 except that a different raw material gas is used from that in step S102. Steps S103A to S105A are performed in the same manner as steps S103 to S105.
[0149] As shown in Table 13 described later, the supply of a raw material gas containing an element X1 as the element X, the supply of a plasma-generated reaction gas, the supply of a raw material gas containing an element X2 as the element X different from the element X1, and the supply of a plasma-generated reaction gas can be repeated to selectively form an oxide film of the element X (to be specific, the elements X1 and X2) on the second film W2 relative to the first film W1, that is, the third film W3. Either the element X1 or the element X2 is a metal element (preferably a transition metal element), and the other is a semiconductor element. By performing both steps S102 and S102A, the crystallization of the third film W3 can be suppressed, and the flatness of the third film W3 can be improved.
[0150] In addition, in Table 13, element X1 is a metal element and element X2 is a semiconductor element, but element X1 may be a semiconductor element and element X2 may be a metal element. In addition, the combination of element X1 and element X2 may be a combination of metal elements or a combination of semiconductor elements. Element X may include element X3 different from elements X1 and X2, or may include three or more different elements. The control unit 100 may also implement the supply of a raw material gas including element X3.
[0151] [Example]
[0152] Next, examples etc. will be described. The following examples 1, 5, and 9 to 17 are examples, and the following examples 2 to 4 and 6 to 8 are comparative examples.
[0153] [Example 1]
[0154] In Example 1, prepare Fig.12 The substrate having the surface of the B film W1-1 and the surface of the SiO film W2-1 on the same plane as shown in Table 1 was subjected to the treatment conditions shown in Table 1. Figure 1 Steps S102 to S105.
[0155]
Table 1
[0156]
[0157] In Table 1, "RF" "ON" means that the gas is plasmatized by high frequency power. "RF" "OFF" means that the gas is not plasmatized. The same is true in the following Tables 2, 3, 5, 7, 8, and 10 to 16.
[0158] As shown in Table 1, in Example 1, TiCl4 gas and plasma-formed O2 gas were alternately supplied to the substrate surface by the plasma ALD method. As a result, Fig.13As shown, the TiO film W3 - 1 is formed selectively on the SiO film W2 - 1 with respect to the B film W1 - 1 .
[0159] [Example 2~Example 4]
[0160] In Examples 2 to 4, preparation and Fig.12 The TiO film was formed on the substrate with the same structure by the thermal ALD method, the thermal CVD method or the plasma CVD method, but the TiO film was formed on the entire surface of the substrate in all cases.
[0161] In Example 2, the supply of TiCl 4 gas and the supply of H 2 O gas not converted to plasma were alternately performed 300 times each with respect to a substrate heated to 350° C. by the thermal ALD method.
[0162] In Example 3, the supply of TiCl 4 gas and the supply of O 3 gas not converted into plasma were simultaneously performed on the substrate heated to 350° C. by the thermal CVD method.
[0163] In Example 4, the supply of TiCl 4 gas and the supply of plasma-formed O 2 gas were simultaneously performed on a substrate heated to 350° C. by a plasma CVD method.
[0164] Comparison of Example 1 with Examples 2 to 4 shows that it is important to use the plasma ALD method in order to form a TiO film selectively on the SiO film relative to the B film.
[0165] [Example 5]
[0166] In Example 5, prepare Fig.33 The substrate having the surface of the BN film W1-5 and the surface of the SiO film W2-5 on the same plane as shown in Table 2 was subjected to the treatment conditions shown in Table 2. Fig.32 processing.
[0167]
Table 2
[0168]
[0169] As shown in Table 2, in Example 5, the supply of TiCl4 gas and the supply of non-plasma-formed O3 gas were alternately performed 300 times each on the substrate surface heated to 400°C by the thermal ALD method. Fig.34 As shown, the TiO film W3 - 5 is formed selectively on the SiO film W2 - 5 relative to the BN film W1 - 5 .
[0170] [Example 6~Example 8]
[0171] In Example 6, prepare Fig.12The Ti film was formed on the substrate of the same structure by the plasma ALD method, but the Ti film was formed on the entire substrate surface. In the plasma ALD method of Example 6, the TiCl4 gas and the plasma-formed H2 gas were alternately supplied to the substrate heated to 350°C.
[0172] In Example 7, prepare Fig.12 The TiN film was formed on the substrate of the same structure by the plasma ALD method, but the TiN film was formed on the entire substrate surface. In the plasma ALD method of Example 7, the TiCl4 gas and the plasma-generated NH3 gas were alternately supplied to the substrate heated to 350°C.
[0173] In Example 8, prepare Fig.12 The TiN film was formed on the substrate of the same structure by the thermal ALD method, but the TiN film was formed on the entire substrate surface. In the plasma ALD method of Example 8, the supply of TDMAT (Ti[N(CH3)2]4) gas and the supply of NH3 gas that was not plasmatized were alternately implemented on the substrate heated to 250°C.
[0174] Comparing Example 1 with Examples 6 to 8, it can be seen that in order to form a Ti-containing film selectively on the SiO film relative to the B film, it is important to convert the reaction gas containing oxygen into plasma and to form an oxide film.
[0175] [Example 9]
[0176] In Example 9, prepare Fig.14 As shown in FIG. 1 , a substrate in which a concave portion is formed on a portion of the surface of the B film W1-9 and only the SiO film W2-9 is exposed at the bottom of the concave portion is subjected to the treatment conditions shown in Table 3. Figure 1 Steps S102 to S105.
[0177]
Table 3
[0178]
[0179] As shown in Table 3, in Example 9, TiCl4 gas and plasma-formed O2 gas were alternately supplied to the substrate surface. Fig.15 As shown, the inside of the concave portion of the B film W1-9 is selectively filled with the TiO film W3-9.
[0180] [Example 10]
[0181] In Example 10, various basement membranes shown in Table 4 were treated under the treatment conditions shown in Table 5. Figure 1Steps S102 to S105 were performed. Then, the thickness of the TiO film formed on the various base films was measured. The results of the thickness measurement are shown in Table 4. In Table 4, "c-Si" is crystallized silicon.
[0182]
Table 4
[0183]
[0184]
Table 5
[0185]
[0186] As is clear from Table 4, a TiO film is formed on a film substantially free of B, whereas a TiO film is not formed on a film containing B. The same tendency is observed under the processing condition where N exceeds 1000 times in step S106 .
[0187] [Example 11]
[0188] In Example 11, various basement membranes shown in Table 6 were treated under the treatment conditions shown in Table 7. Fig. 9 Steps S201 to S205 were then performed under the processing conditions shown in Table 8. Figure 1 Steps S102 to S106 were performed. Then, the thickness of the third film (TiO film) formed on the various base films was measured. Table 6 shows the results of the thickness measurement.
[0189]
Table 6
[0190]
[0191]
Table 7
[0192]
[0193]
Table 8
[0194]
[0195] It is clear from Table 6 that the third film (TiO film) is formed on the SiO2 film and the Mo film, while the third film (TiO film) is not formed on the TiO2 film and the Ru film. By comparing Table 4 and Table 6, it is estimated that the BN film is formed on the TiO2 film and the Ru film, and the BN film is not formed on the SiO2 film and the Mo film. The same tendency is also found under the processing condition where N exceeds 1000 times in step S106.
[0196] [Example 12]
[0197] In Example 12, various basement membranes shown in Table 9 were subjected to the treatment conditions shown in Table 10. Fig. 9Then, the processing conditions shown in Table 11 were implemented. Figure 1 Steps S102 to S106 were performed. Then, the thickness of the third film (TiO film) formed on the various base films was measured. Table 9 shows the results of the thickness measurement.
[0198]
Table 9
[0199]
[0200]
Table 10
[0201]
[0202]
Table 11
[0203]
[0204] It is clear from Table 9 that, compared with the third film (TiO film) not being formed on the SiO2 film, the third film (TiO film) is formed on the TiO2 film, the Mo film, and the Ru film. By comparing Table 4 and Table 9, it is estimated that a BN film is formed on the SiO2 film, and a BN film is not formed on the TiO2 film, the Mo film, and the Ru film. The same tendency was also found under the processing condition that N exceeds 1000 times in step S106. In addition, it is estimated that the difference in the film type of the base film for forming the BN film in Examples 11 and 12 is mainly due to the different types of gases that are plasmatized in step S203. In step S203 of Example 11, NH3 gas is used as shown in Table 7, whereas in step S203 of Example 12, a mixed gas of N2 gas and H2 gas is used as shown in Table 10.
[0205] [Example 13]
[0206] In Example 13, prepare Fig.16 The substrate having the surface of the B film W1-13 and the surface of the SiO film W2-13 on the same plane as shown in Table 12 was subjected to the treatment conditions shown in Table 12. Figure 1 In addition, in Example 13, as shown in Table 12, steps S102A and S103A are implemented after step S103 and before step S104.
[0207]
Table 12
[0208]
[0209] As shown in Table 12, in Example 13, the following supply operation was repeated N times (N=300) by the plasma ALD method: TiCl4 gas, SiCl4 gas, and plasma-formed O2 gas were supplied to the substrate surface in sequence. As a result, Fig.17 As shown, the TiSiO film W3 - 13 is selectively formed on the SiO film W2 - 13 relative to the B film W1 - 13.
[0210] [Example 14]
[0211] In Example 14, prepare Fig.18 The substrate having the surface of the B film W1-14 and the surface of the SiO film W2-14 on the same plane as shown in Table 13 was subjected to the treatment conditions shown in Table 13. Figure 1 In Example 14, as shown in Table 13, steps S102A to S105A are implemented after the nth (n is any natural number greater than 1 and less than N)th steps S102 to S105 and before the n+1th steps S102 to S105.
[0212]
Table 13
[0213]
[0214] As shown in Table 13, in Example 14, the following supply operation was repeated N times (N=300) by the plasma ALD method: TiCl4 gas, plasma-formed O2 gas, SiCl4 gas, and plasma-formed O2 gas were supplied to the substrate surface in order. As a result, Fig.19 As shown, the TiSiO film W3 - 14 is selectively formed on the SiO film W2 - 14 relative to the B film W1 - 14.
[0215] [Example 15]
[0216] In Example 15, prepare Fig.26 The substrate having the surface of the B film W1-15 and the surface of the SiO film W2-15 on the same plane as shown in Table 14 was subjected to the treatment conditions shown in Table 14. Figure 1 Steps S102 to S105.
[0217]
Table 14
[0218]
[0219] As shown in Table 14, in Example 15, Si2Cl6 gas and plasma-formed O2 gas were alternately supplied to the substrate surface by the plasma ALD method. Fig. 27 As shown, the SiO film W3 - 15 is formed selectively on the SiO film W2 - 15 relative to the B film W1 - 15.
[0220] [Example 16]
[0221] In Example 16, prepare Fig.28 The substrate having the surface of the Ru film W4-16 and the surface of the SiO film W2-16 on the same plane as shown in Table 15 was subjected to the treatment conditions shown in Table 15. Fig. 20 Steps S201, S203 and S204, and S102 to S105.
[0222]
Table 15
[0223]
[0224] As a result, in Example 16, Fig.29 As shown, the TiO film W3-16 is selectively formed on the SiO film W2-16 relative to the Ru film W4-16. This is probably because the BN film is formed on the Ru film W4-16, and the BN film is not formed on the SiO film W2-16. The results of Example 16 are also consistent with the results of Example 11 (see Table 6).
[0225] [Example 17]
[0226] In Example 17, prepare Fig.30 The substrate having the surface of the Ru film W4-17 and the surface of the SiO film W2-17 on the same plane as shown in Table 16 was subjected to the treatment conditions shown in Table 16. Fig. 20 Steps S201~S204 and S102~S105.
[0227]
Table 16
[0228]
[0229] As a result, in Example 17, Fig.31 As shown, the TiO film W3-17 is selectively formed on the SiO film W2-17 relative to the Ru film W4-17. This is probably because the B film is formed on the Ru film W4-17, but the B film is not formed on the SiO film W2-17.
[0230] The above describes the embodiments of the film forming method and the film forming device involved in the present disclosure, but the present disclosure is not limited to the above embodiments, etc. Various changes, modifications, substitutions, additions, deletions and combinations can be made within the scope of the claims. These also belong to the technical scope of the present disclosure.
[0231] Description of Reference Numerals
[0232] W: substrate; W1: first film; W2: second film; W3: third film.
Claims
1. A film forming method comprising: Preparing a substrate having a first film containing boron and a second film formed of a material different from that of the first film on a surface thereof, wherein the second film does not substantially contain boron and contains boron in an amount of 5 atomic % or less; supplying a raw material gas containing a halogen and an element X other than a halogen to the surface of the substrate; as well as supplying a plasma-generated reaction gas containing oxygen to the surface of the substrate, The film forming method includes: forming a third film which is an oxide film of the element X selectively on the second film relative to the first film by alternately supplying the source gas and supplying the plasma-generated reaction gas.
2. A film forming method comprising: Preparing a substrate having a first film containing boron and a second film formed of a material different from that of the first film on a surface thereof, wherein the second film does not substantially contain boron and contains boron in an amount of 5 atomic % or less; supplying a raw material gas containing a halogen and an element X other than a halogen to the surface of the substrate; and supplying O3 gas to the surface of the substrate without converting the O3 gas into plasma, The film forming method includes: forming a third film which is an oxide film of the element X selectively on the second film relative to the first film by alternately supplying the source gas and the O 3 gas.
3. The film forming method according to claim 1 or 2, characterized in that: Preparing the substrate includes forming the first film on a fourth film formed of a material different from that of the second film selectively with respect to the second film.
4. The film forming method according to claim 3, characterized in that: Included in order: preparing the substrate having the second film and the fourth film on the surface; forming the first film selectively on the fourth film relative to the second film; forming the third film selectively on the second film relative to the first film; forming the first film again on the fourth film or the first film selectively with respect to the third film; and The third film is formed again on the third film selectively with respect to the first film.
5. The film forming method according to claim 1 or 2, characterized in that: The prepared substrate has a recessed portion on the surface, the first film is exposed only inside the recessed portion, and the first film is exposed at least on the bottom surface of the recessed portion.
6. The film forming method according to claim 1 or 2, characterized in that: The prepared substrate has a recessed portion on the surface, the second film is exposed only inside the recessed portion, and the second film is exposed at least on the bottom surface of the recessed portion.
7. The film forming method according to claim 1 or 2, characterized in that: The element X includes a metal element.
8. The film forming method according to claim 1 or 2, characterized in that: The element X includes a transition metal element.
9. The film forming method according to claim 1 or 2, characterized in that: The element X includes a semiconductor element.
10. The film forming method according to claim 1, characterized in that: include: By repeatedly supplying the raw material gas containing the element X1 as the element X, supplying the raw material gas containing the element X2 as the element X which is different from the element X1, and supplying the reaction gas after the plasma process, an oxide film of the element X, i.e., the third film, is selectively formed on the second film relative to the first film.
11. The film forming method according to claim 1, characterized in that: include: By repeatedly supplying the raw material gas containing the element X1 as the element X, supplying the reaction gas after the plasma process, supplying the raw material gas containing the element X2 as the element X which is different from the element X1, and supplying the reaction gas after the plasma process, an oxide film of the element X, i.e., the third film, is selectively formed on the second film relative to the first film.
12. The film forming method according to claim 2, characterized in that: include: By repeatedly supplying the raw material gas containing element X1 as the element X, supplying the raw material gas containing element X2 as the element X which is different from element X1, and supplying the O3 gas, an oxide film of the element X, i.e., the third film, is selectively formed on the second film relative to the first film.
13. The film forming method according to claim 2, characterized in that: include: By repeatedly supplying the raw material gas containing element X1 as the element X, supplying the O3 gas, supplying the raw material gas containing element X2 as the element X which is different from the element X1, and supplying the O3 gas, an oxide film of the element X, i.e., the third film, is selectively formed on the second film relative to the first film.
14. The film forming method according to any one of claims 10 to 13, characterized in that: Either one of the element X1 and the element X2 is a metal element, and the other one is a semiconductor element.
15. The film forming method according to claim 1 or 2, characterized in that: The element X includes three or more different elements.
16. The film forming method according to claim 1, characterized in that: The supply of the raw material gas and the supply of the reaction gas after the plasma treatment are alternately performed at a temperature of 100° C. to 800° C.
17. The film forming method according to claim 2, characterized in that: The supply of the raw material gas and the supply of the O 3 gas are alternately performed at a temperature of 100° C. to 800° C.
18. A film forming device comprising: A processing container that accommodates a substrate having a first film containing boron on its surface and a second film formed of a material different from that of the first film, wherein the second film does not substantially contain boron and the boron content of the second film is 5 atomic % or less; a holding portion that holds the substrate in the processing container; a supply unit that supplies gas to the surface of the substrate held by the holding unit; a plasma generating unit that converts the gas into plasma; and a control unit that controls the supply unit and the plasma generation unit, in, The control unit performs the following control: by alternately supplying a raw material gas containing a halogen and an element X other than a halogen, and supplying a reaction gas containing plasma-generated oxygen, a third film is selectively formed on the second film relative to the first film, the third film being an oxide film of the element X.
Citation Information
Patent Citations
Method for forming nitride film
JP2017174919A
Tungsten film forming method
CN103132046A
Method of forming metal film and film forming apparatus
CN110616417A
Film forming method and film forming apparatus
CN112582254A
Highly selective silicon oxide / silicon nitride etching by selective boron nitride or aluminum nitride deposition